What is the temperature range of INCOLOY 825?
Incoloy 825 is highly corrosion resistant. It has a high nickel content, sufficient to resist chloride stress corrosion cracking, and a very stable austenitic structure. The molybdenum and copper contents make the alloy resistant to reducing agents and acids. Chromium resists oxidizing conditions, such as nitric acid solutions, nitrates, and oxidizing salts. The alloy is titanium stabilized to resist pitting and intergranular corrosion after fabrication, especially welding, including heating within the critical sensitization temperature range (650°C - 760°C).
Alloy 825 has excellent resistance to sulfuric and phosphoric acid corrosion and is generally the most cost-effective alloy for sulfuric acid service.
Gnee Steel can supply this alloy in plate, sheet, strip, bar, rod, wire, tubing, fittings, fasteners.


Pressure Vessels
Incoloy 825 is approved for use in pressure vessels operating up to 525°C (AS1210, AS4041), 538°C (ASME Boiler and Pressure Vessel Code, Sections I, III, VIII, IX, Case 1936, N-188). At temperatures above ~540°C, brittle phases may form in Alloy 825 and it is not normally used at these temperatures as creep rupture performance is a design factor.
Applications of Incoloy 825
Typical applications for Incoloy 825 alloy include:
Sulfuric acid piping and vessels
Phosphoric acid evaporators
Pickling tank heaters, pickling tanks and equipment
Chemical process equipment
Propeller shafts
Tank trucks
Water heaters
Electrostatic precipitator electrodes
Food, water and seawater thermal vessels
Ammonium sulfate vessels
Expansion bellows
Marine exhaust systems
Power station ash hoppers
Chemical Composition of Incoloy Alloy 825
|
Element |
% |
Element |
% |
|
Nickel |
38.0 – 46.0 |
Carbon |
0.05 max |
|
Chromium |
19.5 – 23.5 |
Manganese |
1.0 max |
|
Molybdenum |
2.5 – 3.5 |
Sulfur |
0.03 max |
|
Copper |
1.5 – 3.0 |
Silicon |
0.5 max |
|
Titanium |
0.6 – 1.2 |
Aluminium |
0.2 max |
|
Iron |
22.0 min (~33%) |
|
|
Tensile Properties of Incoloy Alloy 825
|
Form |
Condition |
0.2% Proof Stress |
Tensile Strength |
Elong |
|
Tube |
Annealed |
440 |
770 |
35 |
|
Tube |
Cold drawn |
880 |
1000 |
15 |
|
Bar |
Annealed |
325 |
690 |
45 |
|
Plate |
Annealed |
340 |
660 |
45 |
|
Sheet |
Annealed |
420 |
760 |
39 |