Element |
Min |
Max |
|
Molybdenum |
15.0 |
17.0 |
|
Chromium |
14.5 |
16.5 |
|
Iron |
4.00 |
7.00 |
|
Tungsten |
3.00 |
4.50 |
|
Cobalt |
-- |
2.50 |
|
Carbon |
-- |
0.02 |
|
Silicon |
-- |
0.08 |
|
Manganese |
-- |
1.00 |
|
Vanadium |
-- |
0.35 |
|
Phosphorus |
-- |
0.03 |
|
Sulfur |
-- |
0.03 |
|
Nickel |
Remainder |
|


Description
Hastelloy C-276 is a nickel-molybdenum-chromium-tungsten alloy that offers excellent general corrosion resistance and good machinability. This alloy should be considered in environments where resistance to hot contaminated mineral acids, organic and inorganic chloride contaminated media, chlorine, formic and acetic acids, acetic acid, acetic anhydride, seawater and brine solutions is required.
Hastelloy C-276 resists the formation of grain boundary precipitates in the weld heat affected zone, making it a candidate for most chemical and petrochemical processing applications in the as-welded condition. The alloy resists general and localized corrosion, including pitting, crevice corrosion and stress corrosion cracking.
Hastelloy C-276 can be easily fabricated by welding, using methods similar to those used for nickel-based alloys.
Corrosion Resistance
Hastelloy C-276 is balanced to provide excellent corrosion resistance for a wide range of chemical process environments. The alloy resists hot contaminated mineral acids, organic and inorganic chloride contaminated media, hypochlorites, chlorine dioxide solutions, formic and acetic acids, acetic anhydride, seawater and brine solutions.
Machinability
Hastelloy C-276 can be forged, hot headed, and impact extruded. Although the alloy is readily work hardened, it can be deep drawn, spun, press formed, or stamped successfully. All common welding methods can be used to weld C-276 alloy, but oxyacetylene and submerged arc processes are not recommended when the fabricated articles are to be used in corrosive service. Special precautions should be taken to avoid excessive heat input.
Welding
Gas tungsten arc welding, gas metal arc welding, shielded metal arc (coated electrode) welding, or resistance welding may be used. Minimum heat input consistent with adequate penetration reduces the likelihood of hot cracking. Oxyacetylene welding should be avoided due to the possibility of carburization. Hastelloy C-276 can be used in most chemical and petrochemical process equipment in the welded condition.
Heat Treatment
Unless otherwise specified, the wrought form of Hastelloy C-276 is supplied in the solution heat treated condition. Alloy C-276 is normally solution heat treated at 2050 °F and rapidly quenched. If possible, hot-formed parts should be solution heat treated prior to final fabrication or installation.