Overview of Hastelloy B series alloys
Hastelloy B series alloys are an important branch of Hastelloy corrosion-resistant alloys. They belong to nickel-molybdenum alloys and are metal materials resistant to corrosion by strong reducing acids (such as hydrochloric acid). The development history, chemical composition, mechanical properties, thermal stability, corrosion resistance and application field of Hastelloy B series alloys are described.
At present, nickel-molybdenum alloys have developed from the first generation Hastelloy B to the second generation Hastelloy B. Hastelloy B-2 to the third generation Hastelloy B-3, Nimofer6629-alloy B-4, Nimofer6224-alloy B-10. The third generation alloy has the advantages of corrosion resistance, thermal stability, processing and forming weldability. The third generation alloy is superior to its predecessors in many aspects such as corrosion resistance, thermal stability, processing and forming, and welding. Due to the insufficient processing performance of Hastelloy B-2, it has gradually withdrawn from the market.


Hastelloy B series alloys have a face-centered cubic lattice structure; only when its organization is pure enough and has the correct crystal structure can it obtain the best corrosion resistance. Because early Hastelloy alloys, such as Hastelloy B and Hastelloy C, need to be fully annealed (i.e., solution treatment) after welding. Otherwise, the corrosion resistance of the heat-affected zone of the weld will be greatly reduced, and welding is a necessary process for the production of most containers, so the early Hastelloy alloys will gradually be improved or eliminated. Based on metallurgical progress (such as the application of argon oxygen decarburization remelting refining technology), the focus of the improvement of the Hastelloy B series alloys is to control carbon and silicon at a very low level, improve the performance of the welding zone, and ensure that the welding zone has the same corrosion resistance as the substrate. In this way, nickel-molybdenum alloys have appeared successively, such as Hastelloy B-2, Hastelloy B-3, and Nimofer6629-alloyB-4. Hastelloy B-2 alloy solves the problem of decreased performance in the weld zone to a certain extent; Hastelloy B-3 solves the problem of easy precipitation of Hastelloy B-2. Hastelloy B-3 solves the disadvantage of Hastelloy B-2 that hardening phase is easy to precipitate, and greatly improves the cold and hot processing performance. Table 1 lists the comparison of commercial grades and standard grades (codes).
1. Nickel-Molybdenum Alloy
1.1 Hastelloy B Alloy
Hastelloy B deformed alloy (UNS No. N10001, nominal composition Ni-28Mo-5Fe-0.3V, patented in 1929), which entered the market in the 1940s, is the earliest solid solution strengthened nickel-molybdenum alloy to enter the market. Due to the high molybdenum content, it has high strength and high corrosion resistance, and is particularly suitable for dealing with strong reducing acids. The main problem of Hastelloy B alloy is that the heat affected zone (HAZ) after welding is always precipitated by second phase precipitates; such precipitates greatly reduce the corrosion resistance of the welded structure. Therefore, Hastelloy B is not suitable for direct use in the post-weld state, because the intergranular corrosion ability of the medium can only be used in the solid solution state.
The solid solution treatment temperature is high and the process is complicated, which is difficult to achieve for some parts and equipment, so the use of Hastelloy B is limited. Therefore, Hastelloy B is no longer used for welding, no longer used as a corrosion-resistant alloy, and is classified as a heat-resistant alloy.
In early high-temperature applications, although Hastelloy B has the characteristics of high yield strength and low thermal expansion coefficient at high temperatures (up to 1095℃), it is limited to use at lower temperatures (650℃) due to its poor oxidation resistance. It is mainly used in old steam turbines and rocket engines. It has now been replaced by the age-hardening high-temperature alloy Haynes242TM. In early chemical corrosion resistant applications, Hastelloy B alloy was strictly limited to reducing acids due to the lack of chromium.
1.2 Hastelloy B-2 alloy
In the 1970s, in order to improve the intergranular corrosion sensitivity of Hastelloy B alloy, the second generation of Hastelloy B-2 (hereinafter referred to as B-2) alloy was developed by reducing the carbon, silicon and iron content. Reducing the carbon and silicon content can significantly reduce the precipitation rate and amount of molybdenum carbide and nickel-molybdenum intermetallic compounds precipitated in the weld and heat-affected zone, thereby greatly reducing the sensitivity to intergranular corrosion, so that it has very good corrosion resistance even in the welded state, so the structure without welding solid solution treatment is also suitable for most chemical applications.
Although B-2 alloy welded vessels do not require post-weld heat treatment under certain media conditions, this fact does not solve the problem because other operations and certain situations require solution treatment, which is necessary and beneficial; the relevant factors are as follows.
(1) B-2 alloy must be solution treated after hot working.
(2) Solution treatment is often required after cold forming to restore plasticity and reduce hardness. Field experience shows that if the cold deformation is less than about 7% of the outer fiber elongation, annealing is generally not required.
(3) Solution treatment of cold-formed materials can reduce the possibility of heat-affected zone (HAZ) embrittlement caused by welding thermal cycles.
(4) Solution treatment can reduce residual stress; residual stress is an important factor in the formation of stress corrosion cracking (SCC). Although stress corrosion cracking is not usually a problem for B-2 alloy, experience has shown that the presence of significant cold deformation in certain environments increases the susceptibility to stress corrosion cracking. Similarly, field experience has shown that deformation of solution-treated parts greater than about 7% of the outer fiber elongation will reduce SCC susceptibility.
(5) Solution treatment can improve the corrosion resistance of the weld fusion zone and heat-affected zone.
Although B-2 alloy has good thermal stability and is not as good as Hastelloy B alloy in manufacturing, B-2 alloy is a pure binary alloy close to Ni-Mo. If it stays in the medium-temperature sensitization zone of 538-870℃ for a short time, Ni4Mo (β-phase) intermetallic compounds will also be quickly precipitated, causing the ductility of the alloy to drop sharply, making it very difficult to process and shape. The 4Mo phase may cause cracking during hot working (forging, hot rolling), cracking during solution treatment, stress corrosion cracking and embrittlement in the heat-affected zone of welding, making B-2 alloy have medium-temperature brittle characteristics. Therefore, B-2 alloy has better thermal stability than Hastelloy B-3 alloy substitutes.
1.3 Hastelloy B-3 alloy
Hastelloy B-3 (hereinafter referred to as B-3) alloy is a third-generation nickel-molybdenum alloy that was launched on the market in the 1990s and patented in 2003. It is an upgraded version of B-2 alloy, the latest achievement of Hastelloy B series alloy. It is the only widely used nickel-molybdenum alloy on the market.
The biggest advantage of B-3 alloy over B-2 alloy is that it can maintain good ductility even after short exposure to medium temperature. Although short exposure to medium temperature is often encountered in manufacturing-related heat treatment processes, and even very short exposure to temperatures such as 700°C can cause severe embrittlement of B-2 alloy, B-3 alloy will not embrittle for a period of time up to several hours, showing significant resistance to such embrittlement, which greatly promotes the ability of the alloy to be processed into complex parts (such as head forming). This is due to the special optimization of the B-3 alloy composition, which slows down the precipitation reaction in the medium temperature zone (600-800℃) to form Ni3Mo (γ phase) intermetallic phase, improving the disadvantage of B-2 that it is easy to precipitate Ni4Mo (β– phase) precipitation phase when passing through medium temperature. The thermal stability of B-3 alloy in the medium temperature zone is much better than that of B-2 alloy, which greatly improves the hot processing performance and has better forming and welding properties.
The uniform corrosion properties of B-3 alloy are the same as those of B-2. B-3 alloy has greatly improved resistance to pitting, stress corrosion cracking, knife corrosion, and weld heat-affected zone corrosion cracking compared to B-2. As with B-2 alloy, B-3 is not recommended for use in acids with iron or copper salts, as this can lead to rapid corrosion failure of the alloy.
When hydrochloric acid comes in contact with iron and copper, it chemically reacts with them to form ferric and divalent copper salts.
Because B-3 alloy is less prone to precipitating deleterious intermetallic phases at moderate temperatures, this improved thermal stability results in greater ductility than B-2 alloy under all types of thermal cycles, thereby minimizing the problems encountered in B-2 alloy fabrication equipment. Therefore, B-3 alloy is suitable for all applications that previously required the use of B-2 alloy and can be used directly in the welded condition.