Introduction to stainless steel grades - performance and characteristics of 253MA
253MA is a heat-resistant austenitic stainless steel grade with excellent high temperature characteristics and good processability. Its high temperature oxidation resistance can reach 1150°C, and its performance is better than that of 310 stainless steel in atmospheres containing carbon, nitrogen and sulfur.
253MA is a trademark of Outokumpu Stainless Steel Company. In the standard grade nomenclature, it is UNS S30815. Other steel mills also produce grades that comply with UNS S30815, including Sirius S15.
The low nickel content of 253MA gives it some advantages over high-nickel alloys and 310 stainless steel in reducing sulfide environments. High contents of chromium, silicon, nitrogen and cerium give the steel good oxide stability, high temperature (creep) strength and excellent resistance to σ phase precipitation.
The austenitic structure gives it excellent toughness, even at freezing temperatures.


Corrosion resistance
Although this grade is not designed to resist corrosion from aqueous solutions, its higher chromium and nitrogen content gives it roughly the same pitting corrosion resistance as 316 stainless steel. 253MA has a high carbon content, so it is prone to sensitization. After high temperature use or processing, the corrosion resistance of aqueous solution media may be reduced.
Heat resistance
Antioxidation: It has excellent antioxidant properties and can reach temperatures as high as 1100°C. At high temperatures, a thin and elastic oxide with strong adhesion will be quickly formed, which has a good protective effect on steel, even under conditions of temperature cycle changes, which is significantly better than 310 stainless steel. The antioxidant performance is best under conditions of non-cyclic changes in temperature.
Resistance to carburization: performs well under oxidizing conditions. If the conditions are reducing, a grade with a higher nickel content should be used.
Anti-sulfurization: In an oxidizing environment (even with only a trace amount of oxygen), it has good resistance to sulfur-containing gases. Reducing gases prevent the formation of protective oxides.
253MA has high strength at high temperatures and is therefore often used in structural and pressure-bearing applications at temperatures around 500°C -900°C.
253MA will undergo sensitization in the temperature range of 425-860°C. This has no effect on high temperature applications, but will result in a decrease in corrosion resistance from aqueous solutions.
heat treatment
Solution treatment (annealing)
Heat to 1050-1150°C and cool quickly. It is recommended that the material be solution treated after 10-20% cold working to obtain the highest creep strength.
Heat treatment cannot harden it
welding
Excellent welding performance, suitable for all standard fusion welding methods. AS 1554.6 pre-qualifies welding with matching 22.12HT electrodes. If lower creep strength is acceptable, 309 filler metal may be used. Pure argon should be used as the protective gas.
machining
Like other austenitic stainless steels, machining requires sharp tools, slow speed, and strong feed.
typical application
Heating furnace components including burners, conveyors, fans, clamps and baskets, rollers, walking beams, radiant tubes, electric heating elements, refractory anchors, hoods, flues, grates, bellows expansion joints, petrochemical and refinery plants of casing hangers.
Performance data specified in standard specifications
ASTM A240/A240M specifies the properties of S30815 flat rolled products (plate, sheet and coil). For other products such as pipes of corresponding specifications, similar but not necessarily the same performance indicators are specified.