Mar 14, 2024 Leave a message

Comprehensive introduction to Inconel718

Inconel718 Ingredient|Performance|Technology|Application

 

Inconel 718 (GH4169)
Overview:
The commonly used 718 alloy can be divided into two categories according to strength, 718 according to the AMS specification, with a yield strength of 150ksi, and 718 according to the NACE specification, with a yield strength of 120ksi.
Alloy 718 is a precipitation hardenable nickel-based alloy that exhibits high yield strength, tensile strength and creep cracking strength in high temperature environments up to 704°C. The age hardening reaction of alloy 718 is relatively slow, so it does not harden with heating and cooling during annealing and welding. Compared with other nickel-based super alloys with added aluminum and titanium, alloy 718 has excellent welding properties.

Inconel718 Ingredient|Performance|Technology|Application

Inconel718 Ingredient|Performance|Technology|Application

Similar brands:
GH4169, GH169 (China),
NC19FeNb (France),
NiCr19Fe19Nb5, Mo3 (Germany),
NA 51 (UK)
Inconel718,UNS NO7718(USA)
NiCr19Nb5Mo3(ISO)
chemical composition:
C≤0.08
Mn≤0.35
Si≤0.015
P≤0.35
S≤0.015
Cr17~21
Ni50~55
Mo2.8~3.3
Cu≤0.3
Ti0.65~1.15
Al0.2~0.8
Fe margin
Nb4.75~5.5
B≤0.006

Physical properties:
Density ρ=8.24g/cm3
Melting temperature range 1260~1320℃

Mechanical behavior:
Tensile strength: 150ksi and above
Yield Strength: 120-145ksi
4D elongation: more than 20%
Area shrinkage (dia≤10"): more than 35%
Area shrinkage (dia>10"): more than 25%
Hardness: 30-40HRC
V-notch impact strength (-59°C or lower):
Average energy: 35ft/lbs (47J) or more
Minimum energy per time: 30ft/lbs (40J)

heat treatment
Solution annealing at 1021-1052°C for 1-2.5 hours, then water quenching. Bars with a diameter less than 3.5" can be water quenched or air cooled. Aged at 774-802°C for 6-8 hours, then air cooled.
Heat treatment needs to be carried out by the steel factory, or under the guidance of the steel factory.
application
Jet engine and high-speed airframe parts such as wheels, turbine blades, gaskets, high-temperature bolts, fasteners, etc.

heat treatment

Method 1: Get the best tensile strength and stress cracking strength

954-982°C, 1 hour, air cooling +718°C, 8 hours, cool to 621°C at 56°C/hour, keep warm for 8 hours, then air cool.

Method 2: Obtain the best room temperature and low temperature tensile strength

Heat treatment at 1066°C for 1-2 hours, air cooling at +718°C for 8 hours, cooling to 621°C at 56°C/hour, heat preservation for 8 hours, and then air cooling.

Processing performance

Thermal processing

The furnace temperature for thermal processing does not exceed 1121°C. If the working temperature is below 593°C, the temperature range of cold working is controlled at 927-1010°C, which can provide forging strength. Avoid prolonged heating in the furnace when forging.

Machine processing

Both annealed and age-hardened states can be machined. The age-hardened state makes it easier to break and cut, and the surface finish is better. For annealed materials, machined tool life is slightly longer.

welding

Both the annealed state and the aged state of 718 can be welded. When welding aged materials, deformation will occur in the area where the weld is heated and softened.


Steel rolling production process flow
1. Bar production line process flow

Billet acceptance→heating→rolling→multi-length shearing→cooling→cutting→inspection→packaging→measurement→warehousing

(1) Billet acceptance = The quality of billet is the key to the quality of finished products and must be inspected and accepted.

①. The billet acceptance procedures include: physical card verification, appearance dimension measurement, surface quality inspection, recording, etc.

②. The acceptance of steel billets is based on billet technical standards and internal control technical conditions. Unqualified steel billets are not allowed to enter the furnace.

(2), billet heating

Billet heating is an important process in the hot rolling production process.

①. The purpose of billet heating

The purpose of billet heating is to improve the plasticity of the steel and reduce deformation resistance to facilitate rolling; the correct heating process can also eliminate or reduce the internal structural defects of the billet. The heating process of steel is directly related to various technical and economic indicators such as steel quality, rolling mill output, energy consumption, and rolling mill life.

②. Three-section continuous heating furnace. The so-called three sections are: preheating section, heating section and soaking section.

The function of the preheating section: use the waste heat of the heating flue gas to preheat the steel billet to save fuel. (Generally preheated to 300~450℃)

The function of the heating section is to reheat the preheated steel billet to 1150~1250℃. It is the main heating section of the heating furnace and determines the heating production capacity of the furnace.

The function of the soaking section is to reduce the temperature difference between the inside and outside of the steel billet and eliminate the black marks on the water-cooled slide to stabilize and evenly heat the quality.

③. Several common defects in billet heating

a. Overheating

When the steel billet is heated at high temperature for a long time, it is easy to overheat. The overheating phenomenon of steel billet is mainly manifested in the excessive growth of steel grains into coarse grain structure, thereby reducing the bonding force between grains and reducing the plasticity of steel.

Overheated steel is prone to cracking during rolling, especially at the corners. When slightly overheated, cracks will occur on the surface of the steel, affecting the surface quality and mechanical properties of the steel.

In order to avoid overheating defects, the heating temperature and heating time must be strictly controlled.

b. Overheated

When the steel billet is heated at high temperature for a long time, it will turn into a coarse crystal structure. At the same time, the low melting point non-metallic compounds on the grain boundaries are oxidized and the crystal structure is destroyed, causing the steel to lose its due strength and plasticity. This phenomenon is called excessive burn.

Over-burned steel can cause severe cracking during rolling. Therefore, overheating is a more serious heating defect than overheating. Overburned steel cannot be saved except by re-smelting it.

Ways to avoid overburning: Reasonably control the heating temperature and the oxidation atmosphere in the furnace, strictly implement the correct heating system and rolling ratio, and avoid excessive temperature.

c. Uneven temperature

This phenomenon is likely to occur when the billet is heated too fast or the output of the rolling mill is greater than the heating capacity. If the temperature of the billet is uneven, the dimensional accuracy of the rolled piece will be difficult to stably control during rolling, and it will easily cause rolling accidents or equipment accidents.

Avoidance methods: Reasonably control the furnace temperature and heating speed; make a good connection between rolling and heating.

d. Oxidation and burning loss

The steel billet is oxidized at room temperature, but the oxidation rate is relatively slow. As the heating temperature increases, the oxidation rate accelerates. When the steel billet is heated to 1100-1200°C, it undergoes intense oxidation under the action of furnace gas to form iron oxide scale. . The production of iron oxide scale increases the heating loss and causes the yield index to decrease.

Measures to reduce oxidation and burning losses: Reasonable heating system and correct operation, and control the atmosphere in the furnace.

e. Decarbonization

When the steel billet is heated, the phenomenon of the surface carbon content decreasing is called decarburization. Steels that are prone to decarburization are generally high-quality carbon structural steel and alloy steel with higher carbon content. These steels have their own special uses. After decarburization, the surface and internal carbon content of the steel are inconsistent, which reduces the strength of the steel and affects its performance. Especially for steels that are required to have high wear resistance, high elasticity and high toughness, the surface hardness and performance will be greatly reduced due to decarburization, and even waste products will be caused.

Control method: Strict heating system, reasonable control of furnace temperature and oxidation atmosphere in the furnace.

(3), rolling

The rolling process is the core of the entire steel rolling production process. The deformation process is completed by billet rolling and becomes the product required by users. The rolling process plays a decisive role in product quality.

The quality of rolled products includes: product geometry, dimensional accuracy, internal structure, process mechanical properties and surface finish, etc. Therefore, the rolling process must formulate corresponding rolling process technical procedures and process management systems based on product technical standards or technical requirements, production product characteristics and production technology and equipment capabilities, as well as production costs and workers' labor conditions. To ensure that the quality of rolled products and technical and economic indicators are optimized.

The rolling process generally consists of one row (group) or two rows (group) of rough rolling mill, intermediate rolling mill and finishing rolling mill. Responsible for the functions of billet section compression, semi-finished product rolling deformation and finished product rolling respectively. The pass pattern of the finished product rolling mill or finishing rolling mill is K1 hole, the pass pattern of the rolling mill before finished product is K2 hole, the pass pattern of the rolling mill before finished product is K3 hole, and so on.

Continuous rolling mill and continuous rolling constant? Continuous rolling mill means that several rolling mill stands are arranged in a row according to the rolling direction. The rolled pieces are rolled and deformed in several rolling mills at the same time. The rolling speed of each stand changes with the length of the rolled piece. The rolling method that increases and keeps the second flow rate of metal in each rolling mill equal or has a slight relationship of stacking steel is called a continuous rolling mill. The continuous rolling mill has high mechanization, automation, rolling speed and rolling precision, so it has high labor productivity and excellent product quality. It is the direction for the transformation and construction of rod and wire rod mills. The rolling process in which the rolling stock passes through each rolling mill with equal volume within unit time is called continuous rolling.

Continuous rolling constant=F1D1N1= F2D2N2= F3D3N3= FnDnNn

In the formula: F-cross-sectional area of rolled piece mm2

D-Roll working diameter mm

N-Roller rotation number (1/min)

(4), finishing

①. Steel cooling

The cooling bed is the main cooling equipment for rolled bar products. The cooling roller is the main cooling equipment for wire products.

The function of the cooling bed and cooling roller table is to cool the high-temperature rolling stock above 800°C to below 150-100°C to restore the inherent physical properties of the steel and facilitate the shearing quality and subsequent process operations.

The cooling method is determined according to the chemical composition, organizational state, use purpose, and possible defects after cooling of the steel. The following cooling methods are determined:

Natural air cooling? Natural air cooling is a cooling method commonly used for steel types such as carbon structural steel, low alloy structural steel, high-quality carbon structural steel, and austenitic stainless steel. This cooling method generally does not affect Physical properties of steel.

Forced rapid cooling? Forced rapid cooling generally uses blowing, spraying, water spraying, etc. The characteristic of the process is to quickly cool the steel to a certain temperature within a certain period of time and then naturally cool it. This cooling method can generally change the internal structure of the steel and affect the physical properties of the steel. Such as improving the mechanical properties of ordinary wires; eliminating network carbides in steel, etc.

Controlled slow cooling? Steel types that are highly sensitive to the stress generated after cooling are generally cooled by controlled slow cooling, such as high-speed tool steel, martensitic stainless steel, high-alloy tool steel and high-alloy structural steel. This cooling method can prevent changes in the steel structure and stress concentration that can cause crack defects.

②.Steel shearing

The purpose of steel shearing: to cut off parts that affect the use (defects) of the steel, such as the head and tail of the steel;

The length required by the user.

Steel shearing equipment is divided into cold shearing and hot shearing. Hot shear is often used for cutting the head, tail or double-length cutting of semi-finished products;

Cold shearing is often used to cut the end, end or length of finished steel.

③,Steel inspection

Steel inspection is a key process to ensure that product quality meets product technical standards and technical conditions. Product inspection usually includes: steel outer dimensions, surface quality, fixed length, weight deviation, process performance, mechanical performance, etc. Steel that does not meet product quality standards must be picked out and classified for disposal.

Common product surface defects and preventive measures: Rod and wire products are usually stipulated that the surface must not have defects such as cracks, folds, ears, scars, delamination and inclusions.

Send Inquiry