Inconel Alloy 740H is a nickel-chromium alloy designed for high-temperature and corrosion resistance, making it suitable for various demanding applications. This alloy is optimized for strength at elevated temperatures and offers excellent resistance to oxidation, sulfidation, and carburization, which are critical properties in many high-temperature industrial processes.
Send Inquiry
Chat Now

As a leading supplier and manufacturer in China, GNEE Steel provides cost-effective nickel-based alloy products.

Product Introduction

Gnee Super Alloy (Tianjin) Co., Ltd. is one of the most professional manufacturers and suppliers of inconel alloy 740h pipe in China. If you're going to wholesale high quality inconel alloy 740h pipe made in China, welcome to get free sample from our factory. Good service and reasonable price are available.

 

INCONEL alloy 740H is a nickel-base, precipitation hardenable superalloy that offers a unique combination of high strength and creep resistance at elevated temperatures along with resistance to coal ash corrosion. The alloy was originally targeted for use as A-USC boiler tubes in the superheater sections of these plants but was then adapted for application as a material for the steam headers to which the boiler tubes are connected. A-USC boiler tubes are conventional sizes [typically 1.5 to 3 inch (38 to 76 mm) outside diameter]. Main steam header pipe sizes occupy a much larger size range, with outer diameter greater than 12 inches (305 mm) and wall thickness likely exceeding 1.5 inches (38 mm). Seamless steam reheat piping, at up to 30 inch (760 mm) outer diameter, is also a feasible product line with INCONEL alloy 740H.

Physical Properties

Density g/cm3 8.05
lb/in.3 0.291
Melting Range °F 2350 - 2484
°C 1288 - 1362
Electrical Resistivity Ω-circ mil/ft 702.7
μ Ω -m 1.168

Mechanical Properties

Test Temperature
°F (°C)
0.2% Yield
Strength,
Ksi (MPa)
Ultimate Tensile
Strength,
Ksi (MPa)
Elongation % Reduction
of
Area %
Transverse Orientation
Room Temp. 105 (724) 154.6 (1066) 23.7 28.1
1292°F (700°C) 82.2 (567) 124.9 (861) 17 23.1
1337°F (725°C) 85.4 (589) 125 (862) 22.8 37.4
1382°F (750°C) 86.4 (596) 118.6 (818) 23.9 28.7
1424°F (775°C) 80.8 (557) 110.1 (759) 22.1 30.7
1472°F (800°C) 86.2 (594) 100.2 (691) 23.5 31.2
Longitudinal Orientation
Room Temp. 107.7 (742) 164.4 (1133) 24.3 39.8
1292°F (700°C) 88.2 (608) 132.3 (912) 31.9 35.7
1337°F (725°C) 87 (560) 126.3 (871) 28.4 34.4
1382°F (750°C) 83.5 (576) 118.2 (815) 22.9 24
1424°F (775°C) 81.8 (564) 111.1 (766) 27.9 37.1
1472°F (800°C) 79.3 (547) 100 (689) 31.5 40.9

 

Inconel Alloy 740H pipeInconel Alloy 740H pipeInconel Alloy 740H pipe

Hot Tags: inconel alloy 740h pipe, China inconel alloy 740h pipe suppliers, inconel alloy cylinder parts, inconel alloy flange fittings, lnconel 718 alloy, inconel alloy spinning process, Inconel 825 Astm Standard, inconel alloy turbine parts

Send Inquiry

whatsapp

Phone

E-mail

Inquiry