UNS S31803 / S32205 Duplex Steel Stainless Steel Coils 0.5 - 14mm Thickness
video

UNS S31803 / S32205 Duplex Steel Stainless Steel Coils 0.5 - 14mm Thickness

The pitting resistance of an austenitic stainless steel can be related directly to alloy composition, where chromium, molybdenum and nitrogen are a weight %. The Pitting Resistance Equivalent Number (PREN) uses the following formula to measure an alloy's relative pitting resistance - the higher the number, the better the pitting resistance.
Send Inquiry
Chat Now

As a leading supplier and manufacturer in China, GNEE Steel provides cost-effective nickel-based alloy products.

Product Introduction

Gnee Super Alloy (Tianjin) Co., Ltd. is one of the most professional manufacturers and suppliers of uns s31803 / s32205 duplex steel stainless steel coils 0.5 - 14mm thickness in China. If you're going to wholesale high quality uns s31803 / s32205 duplex steel stainless steel coils 0.5 - 14mm thickness made in China, welcome to get free sample from our factory. Good service and reasonable price are available.

 

UNS S31803 / S32205 Duplex Steel Stainless Steel Coils 0.5 - 14mm Thickness

Description

Width: 1000-2000mm Length: 6m Or Coil
Thickness: 0.5-14mm Surface: 2B,NO.1 ,1D
Type: Hot Rolled
High Light:

stainless steel coil stock

,

cold rolled stainless steel coil

UNS S31803/S32205 Duplex Steel Stainless Steel Coil 3.0*1500*Coil Duplex Steel Composition

 

 

UNS S31803/S32205 Duplex Steel Stainless Steel Coil 5.0*1500*Coil

We has an extensive inventory of 2205 duplex stainless steel plate in thicknesses from 3/16" (4.8mm) through 6" (152.4mm). The yield strength is about twice that of austenitic stainless steels, thus allowing a designer to save weight and making the alloy more cost competitive when compared to 316L or 317L.

Available thicknesses for Alloy 2205:

3/16" 1/4" 5/16" 3/8" 1/2" 5/8" 3/4" 7/8" 1" 1 1/8" 1 1/4" 1 3/8" 1 1/2"
4.8mm 6.3mm 7.9mm 9.5mm 12.7mm 15.9mm 19mm 22.2mm 25.4mm 28.6mm 31.8mm 34.9mm 38.1mm
 
1 5/8" 1 3/4" 2" 2 1/4" 2 1/2" 2 3/4" 3" 3 1/4" 3 1/2" 4" 5" 6"
41.3mm 44.5mm 50.8mm 57.2mm 63.5mm 69.9mm 76.2mm 82.6mm 88.9mm 101.6mm 127mm 152.4mm

Alloy 2205 (UNS S32305/S31803) is a 22% chromium, 3% molybdenum, 5-6% nickel, nitrogen alloyed duplex stainless steel plate with high general, localized, and stress corrosion resistance properties in addition to high strength and excellent impact toughness.

Alloy 2205 duplex stainless steel plate provides pitting and crevice corrosion resistance superior to 316L or 317L austenitic stainless steels in almost all corrosive media. It also has high corrosion and erosion fatigue properties as well as lower thermal expansion and higher thermal conductivity than austenitic.

Specification Sheet Overview

for Alloy 2205 (UNS S32205/S31803)
A 22Cr-3Mo Stainless Steel:

General Properties

Applications

Standards

Corrosion Resistance

Chemical Analysis

Mechanical Properties

Physical Properties

Structure

Processing

 

General Properties

Alloy 2205 duplex stainless steel plate is a 22% Chromium, 3% Molybdenum, 5-6% Nickel nitrogen alloyed duplex stainless steel plate with high general, localized and stress corrosion resistance properties in addition to high strength and excellent impact toughness.

Alloy 2205 duplex stainless steel plate provides pitting and crevice corrosion resistance superior to 316L or 317L austenitic stainless steels in almost all corrosive media. It also has high corrosion and erosion fatigue properties as well as lower thermal expansion and higher thermal conductivity than austenitic.

The yield strength is about twice that of austenitic stainless steels. This allows a designer to save weight and makes the alloy more cost competitive when compared to 316L or 317L.

Alloy 2205 duplex stainless steel plate is particularly suitable for applications covering the -50°F/+600°F temperature range. Temperatures outside this range may be considered but need some restrictions, particularly for welded structures.


Applications

Pressure vessels, tanks, piping, and heat exchangers in the chemical processing industry

Piping, tubing, and heat exchangers for the handling of gas and oil

Effluent scrubbing systems

Pulp and paper industry digesters, bleaching equipment, and stock-handling systems

Rotors, fans, shafts, and press rolls requiring combined strength and corrosion resistance

Cargo tanks for ships and trucks

Food processing equipment

Biofuels plants

Standards

ASTM/ASME...........A240 UNS S32205/S31803
EURONORM...........1.4462 X2CrNiMoN 22.5.3
AFNOR...................Z3 CrNi 22.05 AZ
DIN.........................W. Nr 1.4462

Corrosion Resistance

General Corrosion
Because of its high chromium (22%), molybdenum (3%), and nitrogen (0.18%) contents, the corrosion resistance properties of 2205 duplex stainless steel plate are superior to that of 316L or 317L in most environments.

Localized Corrosion Resistance
The chromium, molybdenum, and nitrogen in 2205 duplex stainless steel plate also provide excellent resistance to pitting and crevice corrosion even in very oxidizing and acidic solutions.

Isocorrosion Curves

Isocorrosion Curves 4 mpy (0.1 mm/yr), in sulfuric acid solution containing 2000 ppm

Stress Corrosion Resistance
The duplex microstructure is known to improve the stress corrosion cracking resistance of stainless steels.

Chloride stress corrosion cracking of austenitic stainless steels can occur when the necessary conditions of temperature, tensile stress, oxygen, and chlorides are present. Since these conditions are not easily controlled, stress corrosion cracking has often been a barrier to utilizing 304L, 316L, or 317L.

Corrosion Fatigue Resistence
Alloy 2205 duplex stainless steel plate combines high strength and high corrosion resistance to produce high corrosion fatigue strength. Applications in which processing equipment is subject to both an aggresively corrosive enviroment and to cycle loading can benefit from the properties of 2205 duplex stainless steel plate.

Critical Pitting Temperature

Critical Pitting Temperature in 1M NaCl Measured using the Outokumpu Stainless, Inc Pitting Cell

Critical Crevice Corrosion Temperature

Critical Crevice Corrosion Temperature (CCT) in 10% FeCl3•6H2O

General Corrosion in Wet Process Phosphoric Acids

Corrosion Rate, ipy
Grade Solution A, 1401/4F Solution B, 1201/4F
2205 3.1 3.9
316L >200 >200
904L 47 6.3
Composition, wt%
P2O5 HCl HF H2SO4 Fe2O3 Al203 SiO2 CaO MgO
Sol A 54.0 0.06 1.1 4.1 0.27 0.17 0.10 0.20 0.70
Sol B 27.5 0.34 1.3 1.72 0.4 0.001 0.3 0.02 -

Stress Corrosion Cracking Resistance

  Boiling Wick Boiling
Grade 42% MgCl2 Test 25% NaCl
2205 F P P
254 SMO® F P P
Type 316L F F F
Type 317L F F F
Alloy 904L F P or F P or F
Alloy 20 F P P

(P = Pass, F = Fail)

Chemical Analysis

Typical Values (Weight %)

Carbon Chromium Nickel Molybdenum Nitrogen Others
0.020 22.1 5.6 3.1 0.18 S=0.001
PREN = [Cr%] = 3.3 [Mo%] = 16 [N%] ≥ 34

Mechanical Properties

Mechanical Properties at Room Temperature

  ASTM A 240 Typical
Yield Strength 0.2%, ksi 65 min. 74
Tensile Strength, ksi 90 min. 105
Elongation, % 25 min. 30
Hardness RC 32 max. 19

Tensile Properties at Elevated Temperatures

Temperature °F 122 212 392 572
Yield Strength 0.2%, ksi 60 52 45 41
Tensile Strength, ksi 96 90 83 81

Physical Properties

Temperature °F   68 212 392 572
Density lb/in3 0.278 - - -
Modulus of Elasticity psi x 106 27.6 26.1 25.4 24.9
Linear Expansion (68°F-T) 10-6/°F - 7.5 7.8 8.1
Thermal Conductivity Btu/h ft°F 8.7 9.2 9.8 10.4
Heat Capacity Btu/lb ft°F 0.112 0.119 0.127 0.134
Electrical Resistivity Ωin x 10-6 33.5 35.4 37.4 39.4

Structure

The chemical analysis of 2205 duplex stainless steel plate is optimized to obtain a typical 50 a/ 50 g microstructure after solution annealing treatment at 1900°/1922°F (1040°/1080°C).

Chloride Pitting Resistance

The pitting resistance of an austenitic stainless steel can be related directly to alloy composition, where chromium, molybdenum and nitrogen are a weight %. The Pitting Resistance Equivalent Number (PREN) uses the following formula to measure an alloy's relative pitting resistance - the higher the number, the better the pitting resistance.

Processing

Hot Forming

Forming below 600°F is recommended whenever possible. When hot forming is required, the workpiece should be heated uniformly and worked in the range of 1750 to 2250°F. Alloy 2205 duplex stainless steel plate is quite soft at these temperatures and is readily formed. Above this range, 2205 is subject to hot tearing. Immediately below this range, the austenite becomes substantially stronger than the ferrite and may cause cracking, a particular danger to "cold" edges. Below 1700°F there can be rapid formation of intermetallic phases because of the combination of temperature and deformation. Whenever hot forming is done, it should be followed by a full solution anneal at 1900°F minimum and rapid quench to restore phase balance, toughness, and corrosion resistance. Stress relieving is not required or recommended; however, if it must be performed, the material should receive a full solution anneal at 1900°F minimum, followed by rapid cooling or water quenching.

Cold Forming

Alloy 2205 duplex stainless steel plate is readily sheared and cold formed on equipment suited to working stainless steels. However, because of the high strength and rapid work hardening of 2205 duplex stainless steel plate, forces substantially higher than those for austenitic steels are required to cold form it. Also because of the high strength, a somewhat larger allowance must be made for springback.

Heat Treatment

Alloy 2205 duplex stainless steel plate should be annealed at 1900°F minimum, followed by rapid cooling, ideally by water quenching. This treatment applies to both solution annealing and stress relieving. Stress relief treatments at any lower temperature carry the risk of precipitation of detrimental intermetallic or nonmetallic phases.

Machinability

With high-speed steel tooling, 2205 duplex stainless steel plate may be machined at the same feeds and speeds as Alloy 316L. When carbide tooling is used, cutting speeds should be reduced by about 20% relative to the speeds for Alloy 316L. Powerful machines and rigid mounting of tools and parts are essential.

Welding

Alloy 2205 duplex stainless steel plate possesses good weldability. The goal of welding 2205 is that the weld metal and heat-affected zone (HAZ) retain the corrosion resistance, strength, and toughness of the base metal. The welding of 2205 is not difficult, but it is necessary to design welding procedures that lead to a favorable phase balance after welding and will avoid precipitation of detrimental intermetallic or nonmetallic phases.

Alloy 2205 duplex stainless steel plate can be welded by: GTAW (TIG); GMAW (MIG); SMAW ("stick" electrode); SAW; FCW; and PAW.

2205 Code Plus Two and 254 SMO are registered trademarks of Outokumpu Stainless, Inc.

UNS S31803 / S32205 Duplex Steel Stainless Steel Coils 0.5 - 14mm Thickness 3

Hot Tags: uns s31803 / s32205 duplex steel stainless steel coils 0.5 - 14mm thickness, China uns s31803 / s32205 duplex steel stainless steel coils 0.5 - 14mm thickness suppliers, 304 316 316l SS Cold Rolled Steel Coils, 316L Stainless Steel Coil, AISI430 Stainless Steel Foil, 2507 Stainless Steel Coil

Send Inquiry

whatsapp

Phone

E-mail

Inquiry