Ni-718 Alloy Material: Standards, Properties and Applications

What Is Ni-718 Alloy?

Ni-718, also written as Alloy 718 and UNS N07718, is a precipitation-hardening nickel-chromium alloy containing niobium and molybdenum. Niobium, titanium and aluminium are held in a narrow range so that a two-step ageing treatment precipitates a fine gamma-double-prime phase, which provides the strength. The result is a material that combines the high-temperature strength and creep resistance of a nickel-based superalloy with weldability that most precipitation-hardened alloys cannot match. It is produced as bar, billet, forging stock, plate, sheet, strip, wire and seamless tube, and stays non-magnetic in service.

Standards and Grades

Each specification fixes the composition range, the heat treatment and the mechanical property envelope that the supplier must certify on the mill certificate.

ASTM B637 - precipitation-hardening nickel alloy bars, forgings and forging stock; composition and room-temperature mechanical properties.

AMS 5662 - aerospace bar, forgings and rings, solution heat treated and precipitation hardened, including the approval route for flight-critical parts.

AMS 5663 and AMS 5664 - companion aerospace specifications for 718 bar and for 718 plate, sheet and strip.

ISO 15156 / NACE MR0175 - qualification for sour oil and gas service, where resistance to sulphide stress cracking must be demonstrated.

GB/T 14992 - the Chinese designation system, in which the corresponding grade is listed as GH4169.

Chemical Composition and Properties

Nickel forms the balance, chromium provides oxidation and corrosion resistance, and niobium with molybdenum raises high-temperature strength.

Element Typical range (wt. %)
Nickel 50.0 – 55.0
Chromium 17.0 – 21.0
Niobium plus tantalum 4.75 – 5.50
Molybdenum 2.80 – 3.30
Titanium 0.65 – 1.15
Aluminium 0.20 – 0.80
Cobalt 1.00 maximum
Carbon 0.08 maximum
Iron remainder
Property Typical value
Density 8.19 g/cm³ (8190 kg/m³)
Melting range 1260 – 1336 °C
Thermal conductivity at 20 °C about 9 – 11 W/(m·K)
Young's modulus about 200 GPa
Tensile strength, aged 1240 – 1400 MPa
Yield strength, 0.2 % offset, aged 1030 MPa minimum
Elongation, aged 12 – 20 %
Continuous service limit up to about 700 °C (1300 °F)

Processing, Heat Treatment and Fabrication

Ni-718 is normally delivered solution annealed and hardened by the user. The aerospace route is a solution treatment at 954 – 982 °C, ageing at 718 °C for 8 hours, furnace cooling to 621 °C, holding to a total ageing time of 18 hours, then air cooling; heavy forgings may be solution treated at a higher temperature to improve stress rupture life. Hot working runs from about 1120 down to 900 °C. Machining is best performed on solution-annealed material, because the aged alloy is harder and work hardens quickly, and sharp tooling with generous coolant is essential. Welding uses matching nickel-iron-chromium filler classified as AWS ERNiFeCr-2 with inert gas shielding, and the joint is aged afterwards to restore strength.

Applications and Service Environments

Aerospace: turbine discs, compressor blades and casings, exhaust structures, fasteners and high-pressure pump parts.

Oil and gas: wellhead and completion hardware, drill collars, valves and subsea components qualified under ISO 15156.

Nuclear: reactor internals, control rod drive mechanisms and high-load springs.

Cryogenic: parts that must remain ductile at liquefied gas temperatures.

Industrial: extrusion dies, hot forming tooling, bellows and heavy-duty springs.

Deliveries normally carry an EN 10204 3.1 mill certificate together with dimensional, surface and, where required, ultrasonic inspection records.

FAQ

Q: Is Ni-718 the same as GH4169?
GH4169 is the Chinese designation for essentially the same nickel-chromium-niobium alloy, supplied against a different national standard but interchangeable for most industrial applications.

Q: Why is a two-step ageing treatment necessary?
The first step at 718 °C precipitates the strengthening phase and the lower step at 621 °C controls its size and distribution; omitting either step reduces yield strength and fatigue life.

Q: Can Ni-718 be welded and then aged?
Yes. Welding is carried out in the solution-annealed condition with matching filler, and the assembly is aged afterwards so that the weldment recovers most of the parent metal strength.

Q: What is the maximum service temperature?
About 700 °C (1300 °F) for long-term service. Above that level oxidation and creep damage accelerate, and a higher-strength nickel or cobalt alloy becomes the better selection.

Q: Is the alloy suitable for sour oil and gas service?
It is widely used in sour wells, but the product form, hardness limit and heat treatment must be assessed under ISO 15156 before the material is released for that duty.