First, a Clarification About the Two Names
The two designations compared in this article refer to the same precipitation-hardenable nickel-copper grade. Alloy K500 and the nickel-copper K500 material of commerce share one chemical specification and one set of heat treatment routes; the difference between them is nomenclature and mill practice, not metallurgy. Buyers who order round rod should therefore focus on the real variables that change delivered properties: product form, condition of supply, heat treatment, tolerances and the applicable specification. Where genuine differences appear, they are between K500 rod and Alloy 400 rod, or between the annealed and aged conditions of the same grade.
Chemical Composition of Alloy K500 Rod
| Element | Content, % |
|---|---|
| Ni | 63.0 minimum |
| Cu | 27.0 to 33.0 |
| Al | 2.3 to 3.15 |
| Ti | 0.35 to 0.85 |
| Fe | 0.5 to 2.0 |
| Mn | 1.5 maximum |
| Si | 0.5 maximum |
| C | 0.25 maximum |
| S | 0.010 maximum |
Aluminium and titanium are the elements that separate this grade from Alloy 400: they are the source of the gamma-prime precipitates formed during ageing, and their content is held in a narrow band because both strength and ductility depend on it. Sulphur is restricted to 0.010% maximum, tighter than the limit applied to Alloy 400, because the higher-strength grade is less tolerant of low-melting phases at grain boundaries.
Mechanical Properties and the Effect of Condition
| Property | Typical value |
|---|---|
| Density | 8.44 g/cm3 |
| Melting point | 1350 °C (2460 °F) |
| Tensile strength | 1100 MPa (160 000 psi) |
| Yield strength, 0.2% offset | 790 MPa (115 000 psi) |
| Elongation | 20% |
These values describe rod in the hot-worked and aged condition. Rod supplied in the annealed condition is considerably softer and more formable, and rod supplied cold drawn and aged reaches the highest strength levels. Because the properties are generated by heat treatment rather than by a phase that forms spontaneously, the condition of supply stated on the purchase order determines what the finished part will actually do, and a rod that meets the same chemistry can fail a strength requirement if the ageing step is omitted.
Heat Treatment of Alloy K500 Bar and Rod
Annealing is carried out between 850 °C and 1000 °C (1562 °F to 1832 °F), with a holding time of about 3 to 5 minutes per millimetre of section thickness. The optimum annealing temperature is 980 °C (1796 °F). It is not recommended to go above 1000 °C, because excessive grain growth follows and the loss of grain size cannot be recovered by later processing.
The hardening sequence begins with a solution anneal in the range of 925 °C to 1040 °C followed by controlled cooling, which dissolves precipitates left by cold work. Ageing then takes place at about 480 °C to 565 °C for a controlled time, forming the fine gamma-prime particles responsible for the strength increase. Because the grade is more prone to stress corrosion cracking than Alloy 400 when aged, stresses introduced by straightening or machining should be relieved where the service environment is known to be aggressive.
Rod and Bar Size Range
| Product | Size range |
|---|---|
| Round rod and bar | Diameter 3 to 800 mm |
| Flat rod and bar | Thickness 2 to 100 mm, width 10 to 500 mm |
| Hexagonal rod | 2 to 100 mm across flats |
| Tube, seamless | Outside diameter 4 to 219 mm, wall 0.5 to 20 mm |
| Tube, welded | Outside diameter 5.0 to 1219.2 mm, wall 0.5 to 20 mm |
| Plate | Thickness 0.1 to 100 mm, width 10 to 2500 mm |
Applicable Specifications by Product Form
| Form | ASTM | ASME | Other |
|---|---|---|---|
| Bar | B865 | SB865 | - |
| Plate | B865 | SB865 | - |
| Sheet | B865 | SB865 | - |
| Pipe | B165 | SB165 | - |
| Tube | B165 | SB165 | - |
| Fittings | B366 | SB366 | - |
| Forgings | B564 | SB564 | - |
| Welding wire | B164 | SB164 | AWS A5.14 |
Purchasing rod against B865 while a companion forging is ordered to B564 is normal practice, and the two documents must state the same condition of supply so that the finished assembly behaves consistently after machining and ageing.
Frequently Asked Questions
Q: Are Alloy K500 rod and the K500 nickel-copper rod different materials?
No. They are the same precipitation-hardenable nickel-copper grade described under two names, sharing one composition specification and the same heat treatment routes.
Q: What actually changes the properties of K500 rod?
The condition of supply. Annealed rod is soft and formable, while hot-worked and aged or cold-drawn and aged rod develops the full strength of roughly 1100 MPa tensile with 790 MPa yield.
Q: What is the recommended annealing temperature for K500 bar?
Between 850 °C and 1000 °C with 3 to 5 minutes per millimetre of thickness. The optimum is 980 °C, and 1000 °C should not be exceeded to avoid grain growth.
Q: How does K500 rod compare with Alloy 400 rod?
K500 is the precipitation-hardenable version, delivering around three times the yield strength of Alloy 400 with comparable or slightly better corrosion resistance, but with higher sensitivity to stress corrosion cracking when aged.
Q: Which specification covers K500 bar and rod?
ASTM B865 and ASME SB865 cover bar, plate and sheet; pipe and tube are supplied to ASTM B165 or ASME SB165, and forgings to B564 or SB564.
Q: Why are aluminium and titanium controlled so tightly?
They form the gamma-prime precipitates that create the strength during ageing, so the composition window directly determines both the achievable strength and the remaining ductility.