Jan 08, 2024 Leave a message

Datasheet-For-Inconel-601-1-6-(1)-(1).pdf

N06601 Nickel-Chromium Alloy: Composition, Properties and Heat Treatment

Grade Identification and Product Standards

N06601 is a nickel-chromium high-temperature alloy with a chromium content of 21.0 to 25.0% and a controlled aluminium addition that makes the grade far more resistant to high-temperature oxidation than a plain nickel-chromium material. The alloy is known internationally under three designations that all point to the same composition: UNS N06601 in the American system, material number 2.4851 in the European system, and the short form 601 on mill certificates and drawings.

Wrought product is covered by the ASTM B166, B167 and B168 specifications, which between them address rod, bar, wire, seamless pipe and tube, and plate, sheet and strip. Because the grade is not hardenable by precipitation, its properties are delivered by composition plus a solution anneal, and the certificate that matters in practice is the one recording the annealing cycle and the resulting mechanical values.

Chemical Composition

Nickel is quoted here as 58.0 to 63.0% rather than as a minimum such as 72%, because the wrought product specification expresses the balance of the composition as iron. Some published tables reproduce a nickel minimum taken from a marketing datasheet; that figure is not a specification limit and should not be used for acceptance testing.

Element Content, %
Ni 58.0 to 63.0
Cr 21.0 to 25.0
Fe balance
Al 1.0 to 1.7
C 0.10 max
Mn 1.00 max
Si 0.50 max
Cu 1.00 max
P 0.020 max
S 0.015 max

The aluminium range is the defining feature of the grade. It is what allows a protective oxide layer to form quickly, stay adherent, and re-form after thermal cycling, and it is also why the composition cannot simply be treated as a higher-chromium version of a 600-type alloy. Molybdenum is not a deliberate addition here; where a table shows molybdenum as a residual or a dash, that reflects the specification rather than a missing analysis.

Physical and Mechanical Properties in the Annealed Condition

Density: 8.42 g/cm3.

Melting range: 1360 to 1411 °C.

Elastic modulus: 124.7 to 206.5 GPa across the working temperature range, with the highest value at room temperature and the lowest at the top of the range.

Thermal expansion coefficient, 20 to 100 °C: 13.75 µm/m·°C.

Specific heat: 451 J/(kg·K).

These values explain the way the alloy is used. A density close to 8.4 g/cm3 keeps component mass predictable for furnace furniture, and the expansion coefficient in the 13 to 14 µm/m·°C band is low enough for the grade to be paired with austenitic stainless steels and iron-nickel-chromium alloys in mixed fabrications without excessive differential movement.

Property Requirement
Tensile strength, Rm 550 MPa min
0.2% proof strength, Rp0.2 205 MPa min
Elongation, A5 30% min

The combination of a moderate proof strength with high elongation is the reason the grade is chosen for components that must tolerate thermal cycling rather than carry extreme static load. Where higher strength is needed at temperature, the answer is a different grade or a different product form, not a heavier ageing treatment, because this alloy cannot be age hardened.

Heat Treatment and the Role of Aluminium

The alloy is not precipitation hardenable, so it cannot be strengthened by ageing. Cold worked material begins to soften once it reaches roughly 900 °C. Where high-temperature strength is required, solution annealing at 1100 to 1200 °C is recommended, followed by water quenching; air cooling is acceptable for some thicknesses, but the cooling rate must be kept high through the 500 to 800 °C interval to avoid carbide precipitation at the grain boundaries. The aluminium addition then does its work in service: it builds a tightly adherent oxide that resists spalling under repeated thermal cycling, and it also supports resistance to carburization and to sulfur-bearing atmospheres. That combination is why the grade appears in heat treatment furnace components and in diesel engine glow plug parts.

Hot Working, Cold Working and Product Forms

Heating temperature for hot working: 1150 to 1200 °C.

Hot working range: 1050 to 1200 °C.

Light working is possible below 850 °C.

Avoid the 650 to 850 °C range, where the material is prone to cracking.

After hot working, cool rapidly through 500 to 800 °C to avoid carbide precipitation.

Cold workability is good. The grade behaves in much the same way as 310S austenitic stainless steel and as the 800-series iron-nickel-chromium alloys, so tooling, lubricants and intermediate annealing schedules already in use for those materials can generally be carried over with minor adjustment.

Standard delivery conditions for wrought product are as follows.

Seamless pipe: solution annealed and pickled, fixed lengths available.

Plate: solution annealed, pickled and trimmed.

Welded pipe: solution annealed and pickled, with radiographic inspection.

Forgings: annealed and polished.

Bar: supplied in the forged and rolled condition, turned or ground.

Strip: cold rolled, solution softened and descaled.

Wire: solution annealed and pickled, delivered as coils or straight lengths, or as solution annealed straight lengths in a ground and cleaned finish.

Frequently Asked Questions

Q: Can N06601 be hardened by heat treatment?
No. The alloy is not precipitation hardenable, so ageing treatments will not raise its strength. Cold working increases strength but reduces ductility, and solution annealing at 1100 to 1200 °C with a rapid quench is used to restore the soft, uniform condition.

Q: What is the recommended annealing cycle?
Solution anneal at 1100 to 1200 °C and quench in water. Air cooling can be used for some product thicknesses, but cooling must stay fast through 500 to 800 °C so that carbides do not precipitate at the grain boundaries.

Q: Which temperature range should be avoided during hot working?
Avoid working the alloy between 650 and 850 °C, where it is prone to cracking. Heat for hot working at 1150 to 1200 °C, work in the 1050 to 1200 °C range, and carry out light forming below 850 °C if required.

Q: Why does the specification quote nickel as 58.0 to 63.0%?
Because the wrought product specification states iron as the balance element. A common marketing figure of 72% nickel minimum is not a specification limit, and acceptance testing should follow the composition table in the applicable ASTM wrought product standard.

Q: What gives the alloy its oxidation resistance?
The chromium content of 21.0 to 25.0% combined with the aluminium addition of 1.0 to 1.7%. Together they form a protective oxide that resists spalling under severe temperature changes and repeated oxidation, and that also contributes resistance to carburization and sulfur-bearing atmospheres.

Q: How does the grade behave in cold forming?
Cold workability is good and comparable to 310S austenitic stainless steel and the 800-series iron-nickel-chromium grades. However, cold worked material softens from about 900 °C upward, so heavy cold reduction should be followed by a full solution anneal.

Send Inquiry

whatsapp

Phone

E-mail

Inquiry