Chemical composition of Inconel686 corrosion-resistant alloy material Yield strength and process of Inconel686 alloy
Material grade
Inconel686 corrosion resistant alloy
Similar brands
UNS N06686, NS3309,00Cr21Ni58Mo16w4 (national standard brand)
Overview of Inconel686 corrosion-resistant alloy:
Inconel686 is a NI-Cr-Mo solid solution strengthened corrosion-resistant nickel-based alloy. It has excellent corrosion resistance in harsh corrosive environments. It is mainly used for heat exchange in chemical processing, pollution control, papermaking, industrial and municipal waste treatment, etc. devices, reaction vessels, transfer tubes, etc.


Application fields of Inconel686 corrosion-resistant alloy:
1. Thermowells in corrosive atmosphere
2. Chlorine-ethylene monomer production: resistant to chlorine gas, chlorinated hydrogen, oxidation and carbonization corrosion
3. Oxidation of uranium into hexafluoride: resistant to hydrogen fluoride corrosion
4. Fields of production and use of corrosive alkali metals, especially environments using sulfides
5. Use chlorine gas method to prepare titanium dioxide
6. Production of organic or inorganic chlorides and fluorides: resistance to chlorine and fluorine gas corrosion
7. Nuclear Reactor
8. Retorts and components in heat treatment furnaces, especially in carbonizing and nitriding atmospheres
9. For catalytic regenerators in petrochemical production, alloy 686 is recommended for longer service life in applications above 700°C.
Inconel 686 corrosion resistant alloy characteristics:
1. It has good resistance to corrosion by reducing, oxidizing and nitriding media.
2. It has good resistance to stress corrosion cracking at room temperature and high temperature.
3. Has good resistance to corrosion by dry chlorine gas and hydrogen chloride gas
4. It has excellent mechanical properties at zero temperature, room temperature and high temperature.
5. It has good creep rupture resistance and is recommended for use above 700°C.
Physical properties of Inconel686 corrosion-resistant alloy (room temperature):
Density:8.73g/cm3
Melting point:1338~1380
Specific heat capacity 20~700 degrees: 377~519J/kg.K
Resistivity 20~700 degrees: 123.7~127.9.U-(c.m)
Linear expansion 100~600 degrees: 11.97~13.18
Elastic modulus 20~700 degrees: 207~165MPa.
Inconel686 corrosion resistant alloy corrosion resistance:
According to Huntington Specialty Materials of the United States, Inconel 686 alloy, which has unique corrosion resistance properties, has replaced the K-500 alloy used on U.S. Navy ships as connectors. Alloy 686 is a solid solution strengthened alloy that obtains high strength through cold working. In particular, the cold-worked 686 alloy shows outstanding hydrogen embrittlement resistance and corrosion resistance, such as excellent strength, ductility and toughness. The 1.3×33cm (0.5×13 inches) bolts are made from cold-processed 686 alloy rods with a diameter of 38Inm (15 inches) and have a standard R1Tr ji limit tensile strength of 993MPa. These processed bolts are processed into connectors and The middle part of the wedge tension test showed good performance.
Inconel 686 process performance and requirements:
Thermal processing
1. Thermal processing temperature range is 1200℃~900℃, and the cooling method is water quenching or rapid air cooling.
2. To obtain the best corrosion resistance and the most suitable crystal structure, heat treatment must be carried out after heat processing.
3. Materials can be fed directly into the heated furnace
Cold working
1. Cold working materials should be in an annealed or solution heat treated state. The work hardening rate of 686 alloy is close to that of austenitic stainless steel, so similar processing equipment can be selected.
2. Intermediate annealing should be performed during the cold working process
3. When the cold working amount is greater than 5%, the workpiece needs to be solution treated.
4. To reduce material wear, the mold should be made of alloy tool steel, carbide or cast steel.
-----------------------------------
Overview of powder injection molding:
Powder Injection Molding (PIM) consists of two parts: Metal Injection Molding (MIM) and Ceramics Injection Molding (CIM). It is a new method for preparing metal and ceramic parts. Technology, it is a brand-new parts processing technology formed by introducing plastic injection molding technology into the field of powder metallurgy.
The basic process steps of MIM are:
First, select metal powder and binder that meet MIM requirements, and then use an appropriate method to mix the powder and binder into a uniform feed at a certain temperature. After granulation, injection molding is performed to obtain a green part. After degreasing treatment, it is sintered and densified to become the final product (White Part).
Characteristics of powder injection molding technology:
Powder injection molding can produce metal and ceramic parts with complex shapes in one go just like plastic products. This process technology uses the injection method to ensure that the material fills the mold cavity, thus ensuring the realization of highly complex structures of parts. In the past, in traditional processing technology, for complex parts, individual parts were usually produced separately and then assembled; when using PIM technology, integration into a complete single part can be considered, which greatly reduces the production steps and simplifies Processing procedures.
1. Compared with traditional machining and precision casting, the internal structure of the product is more uniform; compared with traditional powder metallurgy pressing/sintering, the product performance is better, the product has high dimensional accuracy and good surface finish, and there is no need to reprocess or just A small amount of finishing is required. The metal injection molding process can directly form thin-walled structural parts, and the shape of the product can be close to or meet the final product requirements. The dimensional tolerance of the parts is generally maintained at the level of ±0.10% to ±0.30%, especially for reducing the cost of hard alloys that are difficult to machine. Processing costs and reducing processing losses of precious metals are particularly important.
2. The geometric shape of the parts has a high degree of freedom, the density of each part of the part is uniform, and the dimensional accuracy is high. It is suitable for manufacturing small parts (0.2~200g) with complex geometric shapes, high precision and special requirements.
3. Alloying has good flexibility and can reduce manufacturing costs for materials that are too hard, too brittle, and difficult to cut, or parts that are segregated or contaminated during raw material casting.
4. The product quality is stable and the performance is reliable. The relative density of the product can reach 95% to 100%, and it can be carburized, quenched, tempered and other heat treatments.
5. It has a wide range of applicable materials, wide application fields, high raw material utilization rate, high degree of production automation, simple process, and can be produced in large quantities continuously. The production process is pollution-free and is produced by a clean process. MIM technology uses molds with a lifespan similar to plastic injection molding molds. Due to the use of metal molds, MIM is suitable for mass production of parts; due to the use of injection machines to form product blanks, production efficiency is greatly improved and costs are reduced, and the injection molded products have good consistency and repeatability, thus providing a good foundation for large-volume production. and large-scale industrial production are guaranteed. Furthermore, one mold with multiple cavities can further improve efficiency and reduce the cost of blank formation.
6. The product has uniform microstructure, high density, high mechanical properties such as product strength, hardness, and elongation, good wear resistance, fatigue resistance, uniform structure, and good performance. During the powder metallurgy pressing process, due to the friction between the mold wall and the powder and the powder and the powder, the pressing pressure is unevenly distributed, which leads to uneven microstructure of the pressed blank, poor material tightness, and low density. Seriously affects the mechanical properties of the product; while MIM is a fluid forming process, the presence of the binder ensures the uniform distribution of the powder, thereby eliminating the uneven microstructure of the blank, thereby making the density of the sintered product close to the theoretical density of the material. As a result, the strength is increased, the toughness is enhanced, the ductility, electrical conductivity, and thermal conductivity are improved, and the overall performance is improved. Like the production of plastic products, it can produce complex-shaped metal, ceramic and other parts in one molding. The product has low cost, good smoothness, surface roughness can reach Ra 0.80 ~ 1.6 μm, high precision, and generally does not require subsequent processing.