Inconel Alloy MA758 Pipe
As a leading supplier and manufacturer in China, GNEE Steel provides cost-effective nickel-based alloy products.
- Send E-mail: ss@gneesteel.com
Gnee Super Alloy (Tianjin) Co., Ltd. is one of the most professional manufacturers and suppliers of inconel alloy ma758 pipe in China. If you're going to wholesale high quality inconel alloy ma758 pipe made in China, welcome to get free sample from our factory. Good service and reasonable price are available.
Inconel Alloy MA758 pipe is a pipe made of special alloy material, and its specific characteristics and applications are as follows:
High temperature performance: The alloy can work at temperatures up to 980℃ and has good creep resistance and fracture resistance. This means that it can maintain structural and performance stability in high temperature environments and is suitable for materials used in high temperature combustion or exhaust systems.
Oxidation resistance: It has good oxidation resistance and can resist oxidation and other corrosive gases at high temperatures. This feature makes it suitable for use in high temperature combustion environments, such as gas turbines.
Physical properties: The density of this alloy material is 8.3g/cm³, the thermal conductivity is 13.4J/ms℃, and the melting point ranges from 1364~1397℃. These physical properties indicate that it is both lightweight and has good thermal conductivity, and has a high melting point, which is suitable for high temperature applications.
Chemical composition: The chemical composition of Inconel Alloy MA758 includes a variety of elements such as nickel, cobalt, chromium, aluminum, and titanium, among which nickel has the highest content. The combination of these elements gives the alloy unique properties, such as nickel increases its structural stability and corrosion resistance.
Physical Properties
| Density | g/cm3 | 8.14 | |
|---|---|---|---|
| lb/in.3 | 0.294 | ||
| Melting Range | °F | 2507 | |
| °C | 1375 | ||
Mechanical Properties
| Mechanical Properties of Bar | |||||||
|---|---|---|---|---|---|---|---|
| Temperature | 0.2% Yield Strength | Tensile Strength | Elongation | ||||
| °C | °F | MPa | ksi | MPa | ksi | % | |
| 20 | 68 | 560 | 81.2 | 949 | 137.6 | 27 | |
| 200 | 392 | 495 | 71.8 | 853 | 123.7 | 22 | |
| 600 | 1112 | 421 | 61.0 | 741 | 107.4 | 23 | |
| 700 | 1292 | 371 | 53.8 | 546 | 79.2 | 29 | |
| 750 | 1382 | 274 | 39.7 | 429 | 62.2 | 41 | |
| 800 | 1472 | 214 | 31.0 | 339 | 49.2 | 47 | |
| 1000 | 1832 | 151 | 21.9 | 173 | 25.1 | 29 | |
| Mechanical Properties of Plate | |||||||
| Temperature | 0.2% Yield Strength | Tensile Strength | Elongation | ||||
| °C | °F | Direction | MPa | ksi | MPa | ksi | % |
| 68 | 20 | Longitudinal | 98.6 | 680 | 149.4 | 1030 | 14 |
| 68 | 20 | Transverse | 100.0 | 690 | 139.2 | 960 | 22 |
| 1800 | 982 | Longitudinal | 31.9 | 220 | 34.8 | 240 | 4 |
| 1800 | 982 | Transverse | 31.9 | 220 | 36.3 | 250 | 6 |
| 2000 | 1093 | Longitudinal | 24.7 | 170 | 26.1 | 180 | 4 |
| 2000 | 1093 | Transverse | 23.2 | 160 | 27.6 | 190 | 5 |



Hot Tags: inconel alloy ma758 pipe, China inconel alloy ma758 pipe suppliers, inconel alloy switch parts, inconel alloy heating system parts, Inconel 718 Bar, Inconel Welded Pipe, inconel piping, inconel alloy modulator parts