Dec 22, 2023 Leave a message

Hastelloy C276: Composition, Corrosion Resistance and Fabrication

What the Grade Is

The alloy designated UNS N10276, commonly called C-276, is a nickel-molybdenum-chromium material with a tungsten addition that sustains useful corrosion resistance in both oxidising and reducing media. It was developed to solve a specific field problem: the intergranular corrosion that appeared in the heat-affected zone of welded equipment made from earlier high-silicon, high-carbon versions of the same alloy family.

The fix was metallurgical. Carbon was reduced to 0.02% maximum and silicon to 0.08% maximum, so that carbide and intermetallic precipitation at grain boundaries is suppressed and the material can be placed in service in the as-welded condition without a post-weld solution anneal.

Chemical Composition

Element Requirement, %
Nickel Balance
Molybdenum 15.0-17.0
Chromium 14.5-16.5
Iron 4.0-7.0
Tungsten 3.0-4.5
Cobalt 2.5 max
Manganese 1.0 max
Vanadium 0.35 max
Silicon 0.08 max
Carbon 0.02 max
Phosphorus 0.04 max
Sulfur 0.03 max

Molybdenum provides resistance to reducing acids; chromium provides resistance to oxidising conditions; tungsten adds further strength to the solid solution and improves performance in chloride-bearing environments. The balance of the three is why the alloy handles mixed-acid and alternating oxidising/reducing duty that defeats leaner stainless grades.

Product Standards

The alloy is ordered by product form against the following specifications:

Product form Specification
Rod and bar ASTM B574
Plate, sheet and strip ASTM B575
Welded pipe ASTM B619
Seamless pipe and tube ASTM B622
Welded tube ASTM B626
Fittings ASTM B366
General requirements for tube ASTM B829

ASME versions of these specifications carry the same technical content and are used when the equipment is to be certified under the ASME Boiler and Pressure Vessel Code.

Corrosion Performance

The alloy is specified for aggressive media where 316L and the duplex grades fail: wet chlorine and hypochlorite service, chlorine dioxide bleach plants, hydrochloric acid in all concentrations at ambient and moderate temperature, sulphuric acid across a wide concentration range, and mixed acids containing chlorides and fluorides. It is also a standard material for flue-gas desulphurisation absorbers, quenchers and outlet ducting, where the combination of acidic condensate, chlorides and high velocity demands resistance to pitting and crevice attack as well as to uniform corrosion.

Three practical limits should be understood:

- Oxidising conditions at elevated temperature, such as strong nitric acid or hot concentrated sulphuric acid with high oxidiser content, exceed the capability of the alloy.
- Hydrochloric acid resistance declines as temperature rises and as oxidisers are absent; above the practical range for the grade, a nickel-molybdenum alloy without chromium is the correct choice.
- Chloride pitting resistance is high but finite, and selection should be confirmed against corrosion-test data or field experience for the actual medium rather than by composition comparison alone.

Fabrication and Heat Treatment

Solution annealing is performed in the 1120-1170 C range with rapid quenching, normally in water. This treatment dissolves phases formed during hot working or welding and restores the corrosion resistance of the surface. Material that has been cold worked above a modest reduction requires an intermediate anneal followed by a final solution anneal.

Fabrication guidance that protects the alloy in service:

- Do not finish hot forming at low temperature; the material should be annealed after deformation.
- Remove all grinding dust, thermal-cut oxide and iron contamination before annealing, otherwise chromium-depleted surface layers form and become preferential corrosion sites.
- Use matching nickel-base filler metal and control interpass temperature; the low carbon and silicon content of the base metal should be matched by the filler metal chemistry.
- Allow for high work-hardening during forming, and design bend radii and forming sequences accordingly.

Typical Applications

Chemical and petrochemical plants use the alloy for reactors, heat exchangers, columns and piping in chloride and acid service. Pollution-control systems use it for absorber towers, mist eliminators, dampers and stack liners. Pulp and paper mills use it in bleach plant washers and chlorine dioxide generators. Pharmaceutical and fine-chemical plants use it where a metal-free product stream and resistance to aggressive cleaning agents are both required. In oil and gas, the alloy is covered by the sour-service requirements of NACE MR0175 / ISO 15156 for applications where carbon and low-alloy steels are not acceptable.

Frequently Asked Questions

Q: Is C-276 the same as UNS N10276?
A: Yes. C-276 is the trade name in common use and UNS N10276 is the standard designation; both appear on mill certificates for the same material.

Q: Does the alloy need heat treatment after welding?
A: In most services, no. The low carbon and silicon contents are designed to prevent grain-boundary precipitation in the heat-affected zone, so the as-welded condition is acceptable. Solution annealing after welding is used for highly aggressive service.

Q: How does it compare with 316L stainless steel?
A: The alloy tolerates chloride pitting, crevice corrosion, hydrochloric acid and wet chlorine conditions that 316L cannot survive at the same concentration and temperature. It is also several times more expensive, so it is normally used as a lining, cladding or in the specific wet locations where 316L fails.

Q: Can it be used in seawater?
A: Yes, provided velocity and aeration are controlled. It resists pitting and crevice attack in seawater well, but stagnant, aerated conditions with deposits should be evaluated for crevice corrosion risk.

Q: What filler metal is used for welding?
A: Matching nickel-molybdenum-chromium filler metal of the same composition class, selected to meet the mechanical and corrosion requirements of the joint; the welding procedure should be qualified for the actual service environment.

Send Inquiry

whatsapp

Phone

E-mail

Inquiry