Nov 10, 2023 Leave a message

Intergranular Corrosion in Stainless Steel: Causes and Prevention

What Is Intergranular Corrosion?

Intergranular corrosion is localised attack that follows the grain boundaries of a metal while the grain bodies themselves stay almost untouched. In austenitic stainless steel the damage is easy to miss from the outside: the surface can remain bright while whole grains drop out of the section, so a welded component may lose most of its load-bearing area before any visible stain appears. The failure mode matters most in welded assemblies, in hot-formed parts and in equipment that has spent time inside a critical temperature band.

Stainless steel resists corrosion because chromium builds a thin, self-repairing passive film on the surface. That film needs roughly 12% chromium or more to stay stable. When the metal immediately beside a grain boundary falls below that level, the boundary becomes the preferred path for attack and the material behaves as if it were a galvanic couple with the grain bodies acting as cathodes.

Sensitisation: Temperature and Mechanism

When an unstabilised austenitic steel is heated into roughly 425 to 815 C, carbon diffuses towards the grain boundaries faster than chromium can follow it. Chromium-rich M23C6 carbides precipitate along those boundaries, and each carbide particle strips chromium from the narrow zone around it. The chromium-depleted zone left behind is the weak link. The same sequence occurs in the heat-affected zone of a weld, where the thermal cycle can leave a sensitised band several millimetres from the fusion line. The practical triggers are:

Service temperature: continuous operation in the 425 to 815 C band is the classic sensitising condition, and thick sections cool slowly enough to stay in it for a long time.

Welding: heat input, interpass temperature and cooling rate together decide whether the heat-affected zone becomes sensitised.

Stress relief: a stress-relief cycle that sits inside the critical band can sensitise a component even when the weld itself is sound.

Time at temperature: only minutes are needed for carbon diffusion at the upper end of the range, so short thermal cycles also count.

Carbon contamination: marking crayons, oils, grease and grinding dust are local carbon sources and produce local sensitisation after annealing.

Grades That Resist Sensitisation

Two routes are used: reduce the carbon so that there is little carbide to form, or add a strong carbide former that keeps carbon away from chromium. The table below summarises the usual choices against ASTM A240 composition limits.

Grade EN number Carbon, max Stabiliser Notes
304 1.4301 0.08% none General purpose; can sensitise if held in the critical band
304L 1.4307 0.030% none Standard choice for welded assemblies in general service
316 1.4401 0.08% none Molybdenum improves chloride pitting resistance
316L 1.4404 0.030% none Default grade for welded chemical and process plant
321 1.4541 0.08% titanium, minimum five times carbon plus nitrogen Retains strength to about 600 C; can show knife-line attack
347 1.4550 0.08% niobium plus tantalum, minimum ten times carbon Stabilised grade for heavy sections and high temperature
High-alloy austenitic, UNS N08904 1.4539 0.020% none Very low carbon with molybdenum, copper and higher nickel for aggressive acids

Low carbon is not a licence to ignore temperature. A 304L component held for a long period near the top of the sensitising range can still precipitate carbides, and cold work accelerates the process. The stabilised grades solve the carbon problem by forming titanium or niobium carbides, but they depend on the stabiliser being taken into solution during the mill anneal; if it is not, the surface can be depleted in stabiliser and knife-line attack follows in strongly oxidising acids.

Test Methods and Acceptance Criteria

ASTM A262, Practice A: oxalic acid etch screening test. The etched structure is classified as step, dual or ditch; a ditch structure indicates sensitisation and calls for a quantitative test.

ASTM A262, Practice B: ferric sulfate and sulfuric acid test, used where a corrosion rate is needed for acceptance.

ASTM A262, Practice C: 65% nitric acid test, also used as a screening test for service in nitric acid.

ASTM A262, Practice E: copper and copper sulfate in sulfuric acid, the Strauss test, widely used for welded samples and in European specifications.

ASTM A763: practices for detecting sensitisation in ferritic and martensitic stainless steels.

ISO 3651-1 and ISO 3651-2: the international equivalents, covering nitric acid medium and sulfuric acid medium respectively.

ASTM G108: electrochemical potentiokinetic reactivation, a fast quantitative method that ranks the degree of sensitisation rather than only detecting it.

Practice A is a screening test only and its result should not be used as a final acceptance criterion. Practices B, C and E give quantitative corrosion rates, and electrochemical reactivation testing is preferred when the extent of sensitisation has to be ranked between samples or evaluated as a heat treatment quality check.

Prevention in Fabrication and Service

Grade selection: use the low-carbon L grades for welded assemblies and the stabilised grades where service temperature is above about 400 C.

Solution annealing: heat to roughly 1040 to 1120 C and cool rapidly enough to keep carbon in solution. Slow cooling through the critical band simply replaces one sensitised structure with another.

Welding practice: limit heat input and interpass temperature, use low-carbon or stabilised filler metal, and avoid wide weaving that extends the dwell time in the critical band.

Heat treatment sequence: perform any stress relief before the final solution anneal where possible, and never stress relieve a stabilised grade inside the carbide precipitation range.

Cleanliness: remove marking ink, crayon, oil and grinding dust before annealing, because these are local carbon sources.

Design: avoid crevices, stagnant zones and dead legs. Once a continuous boundary network has formed, aggressive species concentrated in a crevice attack it far faster than the bulk environment would.

Frequently Asked Questions

Q: At what temperature does stainless steel become sensitised?
Unstabilised austenitic grades are most at risk between about 425 and 815 C. The risk depends on time as well as temperature, and slow cooling through that band after welding or hot forming is the most common cause in service.

Q: Is 304L immune to intergranular corrosion?
No. The low carbon content greatly reduces the risk by limiting carbide precipitation, but very long exposure at the top of the critical range, heavy cold work or carbon contamination can still leave a susceptible structure. A correct solution anneal restores resistance.

Q: What is the difference between stabilised and low-carbon grades?
Low-carbon grades such as 304L and 316L limit carbon to 0.030% so that little carbide can form. Stabilised grades such as 321 and 347 still contain up to 0.08% carbon but add titanium or niobium, which combines with the carbon before chromium is affected.

Q: Which test is used to detect intergranular corrosion?
ASTM A262 Practice A is the usual screening test, with Practices B, C and E available for quantitative acceptance. ASTM G108 electrochemical reactivation testing is used when the degree of sensitisation has to be ranked.

Q: What is knife-line attack?
Knife-line attack is a narrow band of attack in the weld heat-affected zone of stabilised grades such as 321 and 347. It occurs where the stabilising element has been taken into solution and the carbon remains mobile in a narrow band next to the weld.

Q: Can a sensitised component be repaired?
Where the section is still sound, a full solution anneal followed by rapid cooling can restore corrosion resistance, but the geometry and size of the component usually limit this option in the field, so prevention during fabrication is the practical answer.

Send Inquiry