Nickel-based alloy 600/N06600 comprehensive encyclopedia
What is Inconel 600?
Nickel-based alloy: Inconel 600 (UNS N06600) is an early developed nickel-chromium-iron-based solid solution strengthened alloy with good high temperature corrosion resistance and oxidation resistance, good cold and hot processing. Welding process has sufficient hot strength and high plasticity below 700°C. The alloy can be strengthened by cold working, and can also be connected by resistance welding, fusion welding, and brazing. It can be used to produce cold-rolled plates, hot-rolled thick plates, strips, wires, bars, round cakes, ring billets, ring forgings, etc. It is suitable for the production of oxidation-resistant parts that can withstand low loads below 1100°C.
UNS N06600 or W.Nr. Inconel 2, also known as 4816.600, alloy 600, is a nickel-chromium-iron alloy with excellent oxidation resistance and resistance to chloride ion stress corrosion cracking, high-purity water corrosion and caustic corrosion at high temperatures. It is mainly used in furnace parts, chemical and food processing, nuclear engineering and spark electrodes. Inconel 600 (76Ni-15Cr-8Fe) is a basic alloy of the Ni-Cr-Fe series, resistant to reducing environments due to its high nickel content.
Material Grade: Inconel 600 (N06600) Nickel-based alloy.
Similar grades of Inconel 600: GH600, GH3600 (China).


ASTM B167 Inconel 600 Seamless Pipe 1" SCH80
NiCManganeseChromiumSTetraFeMaximum value 0.151170.0150.510Minimum value 72146Inconel 600 Mechanical Properties (UNS N06600)
| Condition | Tensile Strength | Yield Strength (0.2% Offset) | Elongation (min, %) | Reduction of Area | Hardness |
|---|---|---|---|---|---|
| Cold Worked / As Drawn | |||||
| Min (ksi) | 110 | 85 | 10 | - | - |
| Min (MPa) | 760 | 585 | - | - | - |
| Hot Worked / Annealed | |||||
| Min (ksi) | 90 | 40 | 25 | - | - |
| Min (MPa) | 620 | 275 | - | - | - |
Technical standards specify the properties.
Physical Properties of Inconel 600 (UNS N06600)
| Property | Density | Melting Range | Specific Heat | Curie Temperature | Electrical Resistivity | |||||
|---|---|---|---|---|---|---|---|---|---|---|
| Units | lb/in³ | g/cm³ | °F | °C | Btu/lb·°F | J/kg·°C | °F | °C | μΩ·in | μΩ·m |
| Value | 0.306 | 8.47 | 2470-2575 | 1354-1413 | 0.106 | 444 | -192 | -124 | 620 | 1.03 |


ASTM B166 Inconel 600 Round Bar OD = 65mm, Length = 1.9m
Thermal properties of Inconel 600 (UNS N06600):
(1) Melting temperature range: 1370~1430°C.
(2) Thermal conductivity: see Table 2-1.
Table 2-1
| Temperature (°C) | 20 | 100 | 200 | 300 | 400 | 500 | 600 | 700 | 800 | 900 | 1000 |
|---|---|---|---|---|---|---|---|---|---|---|---|
| CTE (10⁻⁶/°C) | 12.85 | 13.94 | 15.15 | 16.62 | 18.71 | 20.72 | 22.40 | 24.49 | 27.0 | 29.51 | 31.60 |
(3) Density of Inconel 600: ρ=8.43g/cm3.
Structure of Inconel 600 (UNS N06600):
When the alloy is treated at 1120°C for 2 hours, only TiN nitrogen and Cr compounds are removed. .7 C.3 type carbides are still Cr structure at 1500°C with 870 hours of long aging. 7 C.3 TiN, the microstructure of the alloy is stable.
Formability of Inconel 600:
This alloy has good hot workability, and the heating temperature for ingot forging is 1110-1140°C. The final forging temperature is not less than 950°C, the slab rolling heating temperature is 1130~1170°C, and the finishing rolling heating temperature is 1090~1130°C. The solution treatment temperature of the finished product is 1010~1050°C.
Inconel 600 (UNS N06600) Specifications
| Form | Standard(s) |
|---|---|
| Metal Type | UNS N06600 |
| Bar | ASTM B166, AMS 5665, DIN 17752 |
| Wire | Not specified |
| Sheet | ASTM B168, AMS 5540, DIN 17750 |
| Plate | ASTM B168, AMS 5540, DIN 17750 |
| Seamless Pipe | ASTM B167 |
| Seamless Tube | ASTM B167 |
| Fittings | ASTM B366 |
| Forgings | ASTM B564, DIN 17754 |
| Welding Wire | FM82/ERNiCr-3 |
| Welding Electrode | FM182/ENiCrFe-3 |
| Equivalent Material | 2.4816 (Werkstoff Nr.) |
Machinability of Inconel 600
Inconel 600 alloy (UNS N06600) can be processed into complex shapes such as pipe fittings, flanges, valve parts, etc. The following is the survey results of the machinability of Inconel 600. The main processing and cutting methods include drilling, boring, turning, grinding, milling, etc.
Characteristics of Inconel 600 (UNS N06600)
Ni-Cr-Fe alloy, solid solution strengthening.
It has good high temperature corrosion resistance and oxidation resistance.
It has excellent hot, cold working and welding properties.
It has sufficient heat resistance and high plasticity up to 700°C.
It can be strengthened by cold working, and can also be connected using resistance welding, welding and welding.