The UNS N04400 nickel-copper alloy is a single-phase solid-solution material that manages seawater and chemical environments with very little maintenance. Its combination of high nickel content and controlled copper addition produces a metal that resists neutral and alkaline salts, performs well in many acids and remains tough over a wide temperature range. The sections below summarise the ingredient side of the grade, the standards that cover each product form and the applications that consume it.
Chemistry and Corrosion Behaviour
The composition is built around a minimum of 63% nickel with 28-34% copper. Iron, manganese, silicon, carbon and sulfur are held to maximum limits so that the structure stays a clean solid solution. That structure is what gives the alloy its freedom from chloride stress corrosion cracking and its resistance to a broad range of reducing and neutral media.
| Grade | C | Mn | Si | S | Cu | Fe | Ni |
|---|---|---|---|---|---|---|---|
| UNS N04400 | 0.30 max | 2.00 max | 0.50 max | 0.024 max | 28.0-34.0 | 2.50 max | 63.00 min |
Behaviour in service follows directly from that chemistry. The alloy is especially resistant to neutral and alkaline salts, handles hydrochloric and hydrofluoric acids well when they are kept free of dissolved air, and gives dependable service in seawater and in high-temperature steam. It is not intended for nitric acid or ammonia, and stagnant water can promote crevice and pitting attack.
Available Forms and Governing Specifications
Every common mill form is standardised, which allows a complete plant to be built from one material family with consistent certification.
| Product form | Specification |
|---|---|
| Sheet, plate and strip | ASTM B127 |
| Seamless pipe and tube | ASTM B165, ASME SB165 |
| Welded pipe and tube | ASTM B725, ASTM B730 |
| Rod, bar and wire | ASTM B164, QQ-N-281 |
| Fittings and accessories | ASTM B366, ASME SB366 |
| Forgings | ASTM B564 |
The same alloy is catalogued as Werkstoff number 2.4360, and equivalent designations exist in the DIN, EN, JIS and GB systems, so imported and domestic documents can be matched without changing the material.
Mechanical and Physical Data
| Property | Value |
|---|---|
| Density | 8.8 g/cm3 (0.318 lb/in3) |
| Melting point | 1350 °C (2460 °F) |
| Tensile strength | 550 MPa (80,000 psi) |
| Yield strength, 0.2% offset | 240 MPa (35,000 psi) |
| Elongation | 40% |
Service temperature reaches 427 °C, and up to 538 °C in sulfur-free oxidising atmospheres, while sub-zero toughness stays adequate for cold climates and cryogenic adjacent duty. Strength beyond the annealed level is obtained by cold working, since the grade does not respond to precipitation hardening.
Applications in Chemical, Petroleum and Marine Plants
In chemical and petrochemical plants the alloy appears as packed columns, pressure vessels, reactors, brine heaters, heat exchangers and salt production equipment. Pumps and valve assemblies, process piping and tube shafts form the moving side of the same duty list, where corrosion resistance and mechanical reliability have to be delivered together.
Chemical and petrochemical: columns, reactors, pressure vessels, brine heaters
Heat transfer: exchanger tube and tube sheets exposed to corrosive media
Salt production and brine handling: evaporators, crystallisers and transfer lines
Marine and offshore: seawater piping, pump and valve trim, shafting
General industry: fasteners, springs and precision machined components
Because a single grade covers plate, pipe, rod, fittings and forgings, fabricators can weld and machine a complete assembly without worrying about galvanic mismatch between the parts.
Fabrication, Welding and Handling Notes
The alloy machines at moderate speeds with generous feed and rigid tooling, and it is readily welded by gas tungsten arc, gas metal arc and shielded metal arc processes. Welding consumables of matching nickel-copper composition are used, joint faces are kept free of sulfur-bearing oils and marking compounds, and heat input is controlled to avoid hot cracking.
Cold forming raises strength and hardness, so inter-pass annealing is scheduled when a large amount of deformation is required. The material also work hardens quickly, which is an advantage in service but means that shearing, forming and machining operations need slightly higher forces than carbon steel of the same thickness.
Frequently Asked Questions
Q: What exactly is the UNS N04400 alloy?
A solid-solution nickel-copper alloy with at least 63% nickel and 28-34% copper, used for seawater, chemical and high-temperature steam service.
Q: Which environments should be avoided?
Nitric acid and ammonia are not recommended, and stagnant water can cause crevice and pitting corrosion, so dead legs and slow-moving pockets are avoided in design.
Q: Which specification applies to each product form?
ASTM B127 for plate, B165 and SB165 for seamless pipe and tube, B725 and B730 for welded product, B164 for bar and wire, B366 for fittings and B564 for forgings.
Q: Can the alloy be heat treated to higher strength?
No. It is a solid-solution grade, so strength increases come from cold working rather than from a precipitation or quench-and-temper treatment.
Q: How does it perform at high temperature?
Continuous service is quoted to 427 °C, rising to 538 °C in sulfur-free oxidising atmospheres, with useful mechanical properties retained at low temperature.
Q: What are the most common applications?
Chemical and petrochemical vessels and columns, heat exchangers, brine heaters, salt production equipment, seawater piping, pump and valve assemblies and shafting.