Short Answer: Which Round Bar Is Better?
Neither Alloy 600 nor Alloy 800 round bar is inherently better; the right choice depends on the service temperature, the mechanical stress and the corrosive environment. Alloy 800 (UNS N08800) offers higher strength together with stronger resistance to oxidation and carburisation, which makes it the more suitable bar for sustained high-temperature work. Alloy 600 (UNS N06600) provides excellent mechanical properties and corrosion resistance across a wider range of environments and is normally the preferred material where high mechanical stress combines with acid, sulphide or saltwater corrosion.
Chemical Composition Compared
The two grades are separated mainly by nickel and chromium. Alloy 600 is a nickel-base alloy with at least 72 % nickel, while Alloy 800 is an iron-base alloy in which nickel is held between 30 % and 35 % and iron forms the balance.
| Element (wt %) | Alloy 600 bar | Alloy 800 bar |
|---|---|---|
| Nickel (Ni) | 72.0 minimum | 30.0-35.0 |
| Chromium (Cr) | 14.0-17.0 | 19.0-23.0 |
| Iron (Fe) | 6.0-10.0 | 39.5 minimum, balance |
| Carbon (C) | 0.15 maximum | 0.10 maximum |
| Manganese (Mn) | 1.0 maximum | 1.5 maximum |
| Silicon (Si) | 0.5 maximum | 1.0 maximum |
| Copper (Cu) | 0.5 maximum | 0.75 maximum |
| Aluminium (Al) | Not deliberately added | 0.15-0.60 |
| Titanium (Ti) | Not deliberately added | 0.15-0.60 |
| Sulfur (S) | 0.015 maximum | 0.015 maximum |
Corrosion and Oxidation Resistance Compared
The comparison is environment-specific rather than absolute, so the table below is written as relative performance.
| Corrosion factor | Alloy 600 bar | Alloy 800 bar |
|---|---|---|
| General corrosion resistance | Very good | Good |
| Resistance to acids such as sulfuric and nitric acid | Good | Moderate to good |
| Chloride stress corrosion cracking | Very high | High |
| Pitting and crevice corrosion | Moderate | Limited to moderate |
| High-temperature oxidation | Good | Very good |
| Carburisation resistance | Moderate | High |
Published maximum service temperatures differ between sources according to whether intermittent or continuous exposure is meant, so the ratings above are best read as comparative service guidance rather than as absolute limits. In practice, Alloy 800 is preferred where oxidation and carburisation dominate, while Alloy 600 is preferred where chloride stress corrosion cracking, sulphide attack or saltwater corrosion is the controlling factor.
Physical and Mechanical Properties Compared
| Physical property | Alloy 600 bar | Alloy 800 bar |
|---|---|---|
| Density | 8.47 g/cm³ | 7.94 g/cm³ |
| Melting range | 1370-1425 °C | 1350-1400 °C |
| Thermal conductivity at 200 °C | 14.9 W/(m·K) | 11.3 W/(m·K) |
| Specific heat capacity | 427 J/(kg·K) | 502 J/(kg·K) |
| Mechanical property | Alloy 600 bar | Alloy 800 bar |
|---|---|---|
| Tensile strength | 550 MPa | 450 MPa |
| 0.2 % yield strength | 240 MPa | 170 MPa |
| Elongation | 40 % | 30 % |
| Hardness | 95 HRB | 85 HRB |
| Modulus of elasticity | 206 GPa | 196 GPa |
These are typical room-temperature values for annealed bar and vary with diameter, processing route and heat treatment.
How to Choose Between Alloy 600 and Alloy 800 Round Bar
Choose Alloy 600 when the controlling risk is chloride stress corrosion cracking, sulphide or saltwater attack, or where the widest possible general corrosion resistance is required.
Choose Alloy 800 when the controlling requirement is sustained high-temperature strength combined with resistance to oxidation and carburisation.
Compare low-temperature behaviour as well: Alloy 600 keeps good mechanical properties at low temperature, while Alloy 800 holds higher strength as the temperature rises.
Check the product form, size and heat treatment, because tensile, yield and hardness values for bar differ from those for plate, strip and tube.
Frequently Asked Questions
Q: Is Alloy 600 round bar better than Alloy 800 round bar?
Neither is universally better. Alloy 600 suits high-stress corrosive environments and stress corrosion service, while Alloy 800 suits high-temperature oxidation and carburisation duty.
Q: What is the difference in nickel content between the two bars?
Alloy 600 contains at least 72 % nickel, whereas Alloy 800 contains 30-35 % nickel with iron as the balance.
Q: Which grade has higher strength?
At room temperature, typical annealed Alloy 600 bar shows higher tensile and yield strength, while Alloy 800 retains its strength better as temperature increases.
Q: Which grade resists chloride stress corrosion cracking better?
Alloy 600 is the stronger performer in chloride-bearing and high-purity water environments, which is why it dominates that class of application.
Q: Which grade is more expensive?
Alloy 600 is normally the more expensive of the two, because its nickel content is far higher.
Q: Can Alloy 600 and Alloy 800 be welded together?
Yes. Both are readily welded by conventional arc processes, and a matching or over-alloyed filler is selected according to the service conditions.