Alloy 625 (UNS N06625) Nickel-Based Alloy: Composition, Standards and Applications

Alloy 625, designated UNS N06625 and known internationally as W.Nr. 2.4856, is an austenitic nickel-chromium superalloy that derives its strength mainly from the solid-solution effect of molybdenum and niobium in a nickel-chromium matrix. The result is high strength and outstanding fatigue resistance from cryogenic temperature up to about 1093 C, combined with corrosion resistance that ranges from strongly oxidising media to mildly reducing service. That combination explains its use in aerospace, chemical processing, flue gas desulfurisation, pulp and paper, marine and pharmaceutical equipment.

Chemical Composition and Designations

The alloy is a single-phase austenitic material with a chromium content high enough for oxidation resistance and a molybdenum plus niobium addition that provides solid-solution strengthening and resistance to pitting and crevice attack.

Element, percent Limit
Nickel 58.0 min
Chromium 20.0 to 23.0
Molybdenum 8.0 to 10.0
Niobium plus tantalum 3.15 to 4.15
Iron 5.0 max
Cobalt 1.0 max
Carbon 0.10 max
Manganese 0.50 max
Silicon 0.50 max
Aluminum 0.40 max
Titanium 0.40 max
Phosphorus 0.015 max
Sulfur 0.015 max

The same alloy is catalogued under the UNS number N06625, the Werkstoff number 2.4856 and several national designations. Buyers should quote the UNS number plus the required product specification rather than a trade name, because composition and testing limits are attached to the specification.

Applicable Standards and Product Forms

ASTM B443 / ASME SB-443 for plate, sheet and strip

ASTM B444 / ASME SB-444 for seamless pipe and tube

ASTM B366 / ASME SB-366 for wrought fittings

ASTM B446 / ASME SB-446 for bar, rod and wire

ASTM B564 / ASME SB-564 for forged fittings and forgings

AWS A5.14 ERNiCrMo-3 wire and AWS A5.11 ENiCrMo-3 covered electrode for welding

Typical stock includes plate from 0.5 mm to 10 mm, bar from 12 mm to 220 mm diameter, and pipe, tube, fittings, flange and wire to order. Material is normally supplied with the original mill certificate, and export documentation such as the customs declaration and certificate of origin can be issued with the shipment.

Physical and Mechanical Properties

Property Value
Density 8.44 g/cm3
Melting range 1290 to 1350 C
Magnetic behaviour Non-magnetic
Tensile strength 758 MPa min
Yield strength, 0.2 percent offset 379 MPa min
Elongation 30 percent min
Hardness HB 150 to 220
Solution annealing 950 to 1150 C, held 1 to 2 hours, then rapid air or water cooling

The annealed condition combines the quoted strength with high ductility and toughness, which is why the alloy is used for components that must absorb thermal cycling, vibration and pressure pulsation without cracking.

Corrosion Resistance and Service Environments

Chloride-bearing organic chemical processes, particularly where acidic chloride catalysts are used

Digesters and bleaching vessels in the pulp and paper industry

Absorption towers, reheaters, flue gas inlet baffles, induced draft fans, agitators, deflectors and ducting in flue gas desulfurisation systems

Equipment and components for sour and acidic gas service

Acetic acid and acetic anhydride reaction generators and sulfuric acid condensers

Pharmaceutical process equipment and bellows expansion joints

The high chromium and molybdenum content gives strong resistance to pitting and crevice corrosion in chloride-contaminated media such as seawater, geothermal water, neutral salt solutions and brine, while the nickel-rich matrix protects against chloride stress corrosion cracking.

Welding, Fabrication and Heat Treatment

Hot and cold forming are both practical, but the alloy work hardens quickly, so cold forming requires generous bend radii and intermediate annealing. For welding, a matching nickel-chromium-molybdenum filler classified as ERNiCrMo-3 is recommended, supplied in 1.0, 1.2, 2.4, 3.2 and 4.0 mm diameters; the corresponding covered electrode is ENiCrMo-3 for shielded metal arc work. Joint faces must be free of oil, marking ink, sulfur-bearing compounds and oxide, and the root should be purged with dry argon. Low heat input and interpass temperature control keep the weld metal and heat-affected zone from losing corrosion resistance. After heavy forming or welding in aggressive service, a solution anneal at 950 to 1150 C followed by rapid cooling restores the metallurgical condition that delivers the corrosion performance quoted above.

Frequently Asked Questions

Q: What is the UNS number of alloy 625 and how should it be ordered?
The alloy is UNS N06625, equivalent to Werkstoff number 2.4856. Order by UNS number plus the product specification, for example plate to ASTM B443 or bar to ASTM B446, so that composition, mechanical property and testing requirements are unambiguous.

Q: What temperature can the alloy withstand?
It holds useful strength and oxidation resistance from cryogenic temperature up to about 1093 C in short-term exposure, with continuous service limits set by the atmosphere and by the mechanical load rather than by one fixed figure.

Q: Which filler metal should be used for welding?
A matching nickel-chromium-molybdenum wire classified as ERNiCrMo-3, or a coated ENiCrMo-3 electrode for shielded metal arc welding. The filler matches the parent metal composition so the weld keeps equivalent corrosion resistance.

Q: Is the alloy suitable for seawater?
Yes. The molybdenum content gives good resistance to pitting and crevice corrosion in chloride-bearing water, and the material is widely used in marine and desalination components.

Q: Is a post-weld heat treatment required?
Normally not for thin sections in mild service. Where the component works in an aggressive electrolyte or has been heavily cold formed, a solution anneal at 950 to 1150 C followed by rapid cooling is the standard restoration treatment.

Q: Is alloy 625 magnetic?
No. The fully austenitic structure is non-magnetic, which is an advantage for instruments and equipment where magnetic permeability must remain low.