Alloy 800H Seamless Pipe and Tube
Alloy 800H is an austenitic nickel-iron-chromium alloy with a controlled carbon content that gives it markedly better creep and rupture strength than the base 800 grade above about 600 °C. It is supplied as UNS N08810 with the DIN equivalent WERKSTOFF NR. 1.4958, and it is normally ordered as seamless pipe or tube for chemical, petrochemical and power plant service.
The alloy keeps a fully austenitic structure at high temperature, resists oxidation and carburisation, and stays tough at low temperature. Its resistance to many aggressive chemical environments, together with good weldability, is why it appears in fired heaters, reformer outlet manifolds and steam piping.
Which ASTM Specification Applies
The specification family is often quoted as one block, but the documents cover different products, and that distinction decides how the pipe is ordered and tested.
| Specification | Product covered |
|---|---|
| ASTM B407 / ASME SB407 | Seamless nickel-iron-chromium alloy pipe and tube |
| ASTM B514 / ASME SB514 | Welded nickel-iron-chromium alloy pipe |
| ASTM B515 / ASME SB515 | Welded nickel-iron-chromium alloy tube |
| ASTM B163 / ASME SB163 | Seamless nickel and nickel alloy condenser and heat exchanger tubes |
For a genuinely seamless pipe or tube of alloy 800H the governing document is ASTM B407. B514 and B515 describe welded products, and B163 is used for seamless condenser and heat exchanger tubes. Describing B515 as a seamless pipe specification, or stating that B515 is also covered by B163, mixes up the welded and the seamless families.
Grades 800, 800H and 800HT
| Grade | UNS | WERKSTOFF NR. | Carbon, % | Distinguishing feature |
|---|---|---|---|---|
| 800 | N08800 | 1.4876 | 0.10 max | General purpose, best creep ductility |
| 800H | N08810 | 1.4958 | 0.05 – 0.10 | Coarse grain, higher creep strength |
| 800HT | N08811 | 1.4959 | 0.06 – 0.10 | Combined aluminium plus titanium limits for maximum rupture strength |
The three grades share one base chemistry; carbon level, grain size and the aluminium plus titanium balance are what separate them. Grade 800H is the usual choice once the metal temperature exceeds roughly 600 °C and creep rather than tensile strength governs the design.
Chemical Composition of Alloy 800H
| Element | Requirement, % |
|---|---|
| Nickel (Ni) | 30.0 – 35.0 |
| Iron (Fe) | 39.5 min |
| Chromium (Cr) | 19.0 – 23.0 |
| Carbon (C) | 0.05 – 0.10 |
| Aluminium (Al) | 0.15 – 0.60 |
| Titanium (Ti) | 0.15 – 0.60 |
| Copper (Cu) | 0.75 max |
| Manganese (Mn) | 1.50 max |
| Silicon (Si) | 1.00 max |
| Sulphur (S) | 0.015 max |
Mechanical and Physical Properties
| Property | Value |
|---|---|
| Density | 7.94 g/cm3 |
| Melting range | 1350 – 1400 °C |
| Tensile strength | 520 MPa (75,000 psi) |
| Yield strength, 0.2 % offset | 205 MPa (30,000 psi) |
| Elongation | 30 – 35 % |
Solution annealing is the mill treatment. The pipe is held at roughly 980 °C and cooled rapidly enough to keep carbon in solution. Slow cooling or a low-temperature anneal can sensitise the alloy and reduce its resistance to intergranular corrosion in aqueous service, so the annealing record forms part of the mill certificate.
Size Range and Pressure Ratings
| Item | Range |
|---|---|
| Nominal size | 15 NB – 150 NB |
| Outside diameter | 6.35 – 254 mm |
| Wall thickness | 0.6 – 20 mm |
| Schedules | SCH10, SCH20, SCH30, SCH40, SCH60, SCH80, SCH120, SCH140, SCH160, STD, XS, XXS |
| Lengths | Single random, double random, cut length |
Cold-drawn tube is rated hydraulically as well as by wall thickness. Representative working pressures for the small tube sizes run from about 7900 psig on 1/8 in outside diameter with 0.028 in wall down to about 2200 psig on 1 in outside diameter with 0.120 in wall, and the full table is used when the tube replaces a pipe run in an instrument or sampling line.
Applications
Chemical and petrochemical plants, including reformers and cracker furnaces
Heat exchangers, reactors and process piping
Oil and gas gathering and processing lines
Power generation boilers and superheaters
Nuclear fuel reprocessing systems
Steam and exhaust piping in high-temperature service
Frequently Asked Questions
Q: Is alloy 800H seamless pipe covered by ASTM B515?
No. B515 covers welded tube. Seamless pipe and tube of the same alloy is covered by ASTM B407, and seamless condenser and heat exchanger tube by ASTM B163.
Q: What is the difference between 800, 800H and 800HT?
They share one base chemistry but differ in carbon range, grain size and the aluminium plus titanium balance; 800H and 800HT give higher creep and rupture strength at high temperature.
Q: How is the pipe heat treated?
Seamless product is annealed in the region of 980 °C and then cooled rapidly. The cycle and cooling method are recorded on the mill certificate because they affect intergranular corrosion resistance.
Q: At what temperature does 800H become the better choice?
Above roughly 600 °C creep and rupture strength start to govern the design, and the coarse-grained 800H or 800HT grade is selected instead of plain 800.
Q: Which product forms are available?
Seamless and welded pipe and tube, U-bends, coiled and pancake coils, hydraulic tube, plus round and rectangular tube for structural and support use.